摘要

The phase transformations in the Fe-8.0Al-31.5Mn-1.05C,
Fe-9Al-30Mn-2.0C, Fe-9.0Al-30.5Mn-(0-2.5)Si-1.2C, Fe-8Al-5Ni-2C,
have been examined by means of OM, STEM and EDS. As a result the
following conclusions have been presented.(1) When the Fe-8.0
Al-31.5Mn-1.05C alloy was solution heat-treated and quenched,
the microstructure was single-phase austenite. After being
aged at 550℃, a γ→γ+κ-phase transition had occurred on
the grain boundaries and twin boundaries. This result is quite
different from that observed by other workers in the Fe-(4.9-11)
wt pct Al-(28.5-34.3) wt pct Mn-(0.50-1.62)wt pct C alloys.
In their studies, they found that when the alloy was aged
at temperatures ranging from 550℃to 650℃, aγ→α+β-Mn, γ→
α+β-Mn+κand γ→ β-Mn reaction occurred on the grain
boundaries.(2) In the as-quenched condition, the microstructure
of Fe-9Al-30Mn-2.0C alloy was a mixture of (γ+κ'-
carbide). When the alloy was aged at temperatures ranging from
550 ℃ to 750 ℃, fine κ'-carbides existing in the as-
quenched austenite matrix grew preferentially along <100>
directions and a γ→γ+κ-phase transition had occurred on the
grain boundaries. When the aging temperature was in the
range from 850℃ to 950℃, both coarse κ' and fine κ'-
carbides could be observed within the austenite matrix . In the
grain boundaries, a γ→ γ+coarse κ-carbide + fine κ-
carbide transition had occurred on the grain boundaries. It
is worthy to note that the κ-phase carbide has L'12-type
structure at 650℃ or below and has an L12 type structure at
750℃ or above. These results are quite different from those
reported by other workers in various Fe-Al-Mn-C alloys.(3) The
effects of Si addition on the as-quenched microstructure of
Fe-9.0Al-30.5Mn-1.2C alloy have been investigated. The
results indicated that Si addition would enhance the κ'-
carbides to precipitate coherently within the austenite
matrix during rapid quenching by spinodal decomposition.
With increasing the Si content to 1.5wt.%, (α+ D03) phases were
also formed on the austenite grain boundaries in addition to
the formation of the κ'-carbides within the austenite
matrix. The D03 phase was formed during quenching by a α→B2→
D03 continuous ordering transition. (4) In the as-quenched
condition, the microstructure of the alloy was austenite phase
containing fineκ'-carbides. Theκ' carbides were formed
during quenching by a spinodal decomposition. When the as-
quenching alloy was aged at 550℃for short times, theκ'-
carbides grew along <100> directions. After prolong aging at
this temperature, aγ→α+B2+κ reaction occurred on the
austenite grain boundary. This result is different from that
observed by Choo and Kim in the same alloy.
None
顯示完整詮釋資料 統計資料

引用此條目

黃志能 (1997). 鐵鋁錳碳, 鐵鋁錳矽碳和鐵鋁鎳碳合金相變化. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/14532

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/14532