鎢化鈦與鈦鎢氮化物薄膜應用於銅金屬化之擴散阻障層特性研究
顯示簡易詮釋資料 統計資料| 欄位 | 內容 | 語言 |
|---|---|---|
dc.contributor.advisor |
張立 | |
dc.contributor.advisor |
Li Chang | |
dc.contributor.author |
陳種發 | |
dc.contributor.author |
Joong-Fa Chen | |
dc.contributor.college |
工學院 | |
dc.contributor.committee |
||
dc.contributor.committee |
||
dc.contributor.department |
材料科學與工程學系所 | |
dc.contributor.studentid |
8818548 | |
dc.date.NCLavailable |
||
dc.date.USTavailable |
||
dc.date.issued |
2001 | |
dc.date.issuedROC |
90 | |
dc.date.paperavailable |
立即公開 | |
dc.date.schoolyear |
89 | |
dc.description.abstract |
摘 要 在目前極大型積體電路的發展中,以銅作為導線引起越來越多人的注意,且進入深次微米製程,以銅取代鋁,做為金屬導線材料已成為必然的趨勢。為了克服銅與矽基材間相互擴散的問題,必須在銅與矽間鍍上具有低電阻係數、高熱穩定性及良好界面附著性的擴散阻障層。本實驗主要是在探討以TiW與TiWN薄膜做為銅與矽之間擴散阻障層的反應,由擴散、相變化的觀點來討論其變化。所採用的鍍膜結構如下: Si3N4(20nm)/Cu(100nm)/TiW(20nm)/SiO2(20nm)/Si Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si Si3N4(20nm)//TiWN(20nm)/SiO2(20nm)/Si 在改變的氮/氬比例下以濺鍍法來沉積阻障層,再濺鍍銅膜,並利用PECVD沉積一層Si3N4,目的是避免退火過程中造成銅表面的氧化。對試片做450~800℃/ 30分鐘的氮氣氣氛退火處理,以四點探針量測片電阻,掃瞄式電子顯微鏡(SEM)用來觀察銅膜表面型態,歐傑電子能譜儀(AES)做成分縱深分析,X光繞射儀(XRD)做相的鑑定,並利用穿透式電子顯微鏡(TEM)做鍍膜截面的觀察,分析各層結構的變化。 研究結果顯示這幾種不同的結構在退火後有不同的行為,Cu/TiW/SiO2/Si結構與Cu/TiWN/SiO2/Si 結構(Ar-10%N2)分別在650℃與800℃/30分鐘退火後片電阻值明顯上升,約為976 與1116 mΩ/□,阻障層與銅膜產生銅-鈦析出物,顯示阻障層已經失去了阻絕銅擴散的能力。Cu/TiWN/SiO2/Si結構(Ar-16.6%N2與Ar-30%N2)在700℃退火後片電阻值有明顯的上升,其原因為表面銅膜產球化不連續的結團所導致。 由實驗結果可知Cu/TiWN/SiO2/Si 結構(Ar-16.6%N2),電阻值低,且具有高的熱穩定性。因退火過程中,TiWN阻障層產生變化,其變化原因將於本文中討論,氮元素在其中扮演了重要的角色。 | |
dc.description.abstract |
Abstract Copper has attracted a lot of attention as a promising interconnect material in the fabrication of deep sumbmicro devices of ultra-large scale integration circuit devices due to its lower resistivity and better properties than conventional Al alloys. Since Cu diffuses fast in Si and forms deep-level trap defects, a proper diffusion barrier is needed. The barrier should have low resistivity, high thermal stability, and good adhesion with Cu and substrate. In this study, we investigate the diffusion barrier properties of TiW and TiWN thin films for Cu metallization in ULSI circuit device. The following structures are used: Si3N4(20nm)/Cu(100nm)/TiW(20nm)/SiO2(20nm)/Si Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si Si3N4(20nm)//TiWN(20nm)/SiO2(20nm)/Si Copper and barriers were deposited by DC sputtering. The barriers were deposited by varying the N2/Ar ratio. Subsequently, a Si3N4 was deposited by plasma enchanced chemical vapor deposition (PECVD), in order to prevent the Cu surface from reacting with oxygen during annealing process. Annealing was carried out in nitrogen ambient at temperatures from 450 to 800 ℃ for 30 min. Sheet resistance was measured by a four-point probe method. Copper surface morphplogy(AES)was inspected by scanning electron microscopy(SEM). Auger electron spectroscopy was used to evaluate the inter-diffusion across the interface by the compositional depth profile. The phase identification of layers was performed by XRD. The microstructure was investigated by cross-sectional transmission electron microscopy(TEM)with X-ray energy dispersive spectroscopy(EDS).Sheet resistance measurement and microstructural characterization showed that these structures have different behaviors after annealing. The barriers of Cu/TiW/SiO2/Si and Cu/TiWN/SiO2/Si structures deposited at the condition Ar-10%N2 mixtures were failed after annealing at 650℃ and 800℃ for 30 min due to the formation of copper-titanium related precipitate in Cu film. Sheet resistances of Cu/TiWN/SiO2/Si structures fabricated at the conditions of Ar-16.6%N2 and Ar-30%N2 after 700℃ annealing due to the spheroidization of Cu films. From these results, the structure of Cu/TiWN/SiO2/Si fabricates at the condition of Ar-16.6%N2 has low resistivity, high thermal stability. It is suggested that nitrogen plays important roles on the thermal stability. | |
dc.description.abstractopendate |
||
dc.description.degree |
碩士 | |
dc.description.tableofcontents |
目錄 頁次中文摘要------------------------------------------------------ i英文摘要-----------------------------------------------------iii誌謝---------------------------------------------------------- v目錄----------------------------------------------------------vi表目錄------------------------------------------------------viii圖目錄--------------------------------------------------------ix第一章、緒論1.1、 銅金屬化---------------------------------------------11.1.1、 內連線的發展趨勢-------------------------------------11.1.2、 銅金屬的特性-----------------------------------------11.1.3、 擴散阻障層材料的選擇---------------------------------3第二章、文獻回顧-2.1、銅的應用—積體電路(IC)----------------------------------52.1.1、IC的發展趨勢--------------------------------------------52.1.2、內連線材料的選擇----------------------------------------62.1.3、銅的沉積技術--------------------------------------------82.1.4、銅導線的鑲嵌技術---------------------------------------102.2、銅製程的擴散阻障層---------------------------------------102.2.1、擴散阻障層選用的趨勢-----------------------------------102.2.2、擴散阻障層材料的比較-----------------------------------122.2.3、擴散阻障層熱穩定性的比較-------------------------------142.2.4、TiW與TiWN應用於擴散阻障層的研究------------------------152.2.5、實驗設計-----------------------------------------------20第三章、實驗步驟與方法3.1、製程-----------------------------------------------------353.1.1、試片清洗-----------------------------------------------353.1.2、薄膜濺鍍-----------------------------------------------363.1.3、熱處理-------------------------------------------------373.1.4、濕蝕刻-------------------------------------------------373.2、材料分析與量測技術---------------------------------------373.3、TEM試片製備----------------------------------------------41第四章、結果與討論4.1、X光繞射分析(XRD)---------------------------------------494.2、片電阻量測(Sheet resistance)---------------------------504.3、場發射電子顯微觀察(FE-SEM)-----------------------------524.4、歐傑電子能譜縱深分析(AES)------------------------------534.5、穿透式電子顯微觀察(TEM)--------------------------------544.6、Si3N4/Cu/TiW與Si3N4/Cu/TiWN阻障結構的比較----------------684.7、TiWN與其他阻障結構的比較---------------------------------71第五章、結論-------------------------------------------------101第六章、未來研究與建議方向-----------------------------------103參考文獻-----------------------------------------------------104附錄---------------------------------------------------------114表目錄 頁次表2-1、IC發展趨勢預測-----------------------------------------22表2-2、內連接導線材料相關性質的比較---------------------------25表2-3、各種沉積銅膜技術的比較---------------=-----------------26表2-4、各種擴散阻障層材料的電阻係數---------------------------29表2-5、各種擴散阻障結構的熱穩定性比較-------------------------30表4-1、不同結構銅的I (200) / I (111)和I (220) / I (111)之實際比值------------------------------------------------------------66表4-2、銅膜與擴散阻障層的XRD(JCPDS)相關資料-----------------67表4-3、TiW 阻障層隨溫度變化與晶格常數的關係-------------------68表4-4、TiWN Ar-10N2阻障層隨溫度變化與的晶格常數的關係---------68表4-5、TiWN Ar-16.6N2阻障層隨溫度變化與晶格常數的關係---------69表4-6、TiWN Ar-30N2阻障層隨溫度變化與晶格常數的關係-----------69表4-7、不同結構的原始片電阻與電阻變化溫度的比較---------------70圖目錄 頁次圖2-1、閘級延遲及導線延遲與元件尺寸的關係圖-------------------24圖2-2、突穿現象示意圖-----------------------------------------24圖2-3、銅-矽(Cu-Si)二元相圖---------------------------------26圖2-4、濺鍍中簡單粒子行為示意圖-------------------------------27圖2-5、Dual Damascene製程流程圖-------------------------------28圖2-6、擴散阻障層材料選用的趨勢圖-----------------------------27圖2-7、典型的MOS電容的截面結構圖------------------------------29圖2-8、典型的擴散阻障層變化圖---------------------------------31圖2-9、鈦-鎢(Ti-W)二元相圖----------------------------------31圖2-10、鈦-鎢-氮(Ti-W-N)三元相圖----------------------------32圖2-11、鈦鎢氮化物電阻值與氮含量的關係圖----------------------33圖2-12、鎢化鈦電阻值與化學組成的關係圖------------------------33圖2-13、Ti-W濺鍍產率圖----------------------------------------40圖2-14、實驗結構圖--------------------------------------------40圖3-1、RCA clean的流程圖--------------------------------------43圖3-2、濺鍍方法示意圖-----------------------------------------44圖3-3、PECVD的反應示意圖--------------------------------------44圖3-4、四點探針的量測示意圖-----------------------------------45圖3-5、AES能譜儀原理示意圖------------------------------------45圖3-6、TEM的基本構造圖----------------------------------------46圖3-7、TEM試片製作流程圖--------------------------------------47圖3-8、實驗流程圖----------------------------------------------55圖4-1、Si3N4(20nm)/Cu(100nm)/TiW(20nm)/SiO2(20nm)/Si結構450~800℃退火XRD繞射疊圖------------------62圖4-2、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-10%N2) 450~800℃退火XRD繞射疊圖-----------------63圖4-3、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)450~800℃退火XRD繞射疊圖------------------64圖4-4、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si 結構(Ar-30%N2) 450~800℃退火XRD繞射疊圖-------------------65圖4-5、Cu(100nm)/TiW(20nm)/SiO2(20nm)/Si結構Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-10%N2)Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2 )Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-30%N2)不同結構在不同退火溫度下的相對片電阻變化率-------------72圖4-6、TiWN/SiO2/Si結構(Ar-16.6%N2)在不同退火溫度下的電阻係數變化率--------------------------------------------------------72圖4-7、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-10%N2)(a)as-deposited (b)650℃(c)700℃ (d)800℃退火SEM照片-----------------73圖4-8、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)(a)as-deposited (b)650℃(c)700℃ (d)800℃退火SEM照片-----------------74圖4-9、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-30%N2)(a)as-deposited (b)650℃(c)700℃ (d)800℃退火SEM照片-----------------75圖4-10、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(a)as-deposited (b)600℃(c)650℃ (d)700℃(e)750℃ (f)800℃退火歐傑縱深份佈圖----------76圖4-11、Si3N4(20nm)/Cu(100nm)/TiW(20nm)/SiO2(20nm)/Si結構(a)as-deposited XTEM照片及SAD繞射圖(b)500℃退火 XTEM照片(c)550℃退火 XTEM照片-(d)800℃退火 XTEM明視野、暗視野照片及SAD繞射圖-------79圖4-12、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-10%N2)(a)as-deposited XTEM照片及SAD繞射圖(b)600℃退火 XTEM照片及SAD繞射圖(c)700℃退火 XTEM照片及SAD繞射圖(d)800℃退火 XTEM明視野、暗視野照片及SAD繞射圖-------83圖4-13、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)(a)as-deposited XTEM照片及SAD繞射圖(b)500℃退火 XTEM照片(c)600℃退火 XTEM照片(d)650℃退火 XTEM照片及SAD繞射圖(e)700℃退火 XTEM照片(f)750℃退火 XTEM照片(g)800℃退火 XTEM照片及SAD繞射圖---------------------88圖4-14、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-30%N2)(a)as-deposited TEM照片及SAD繞射圖(b)800℃退火 TEM照片及SAD繞射圖----------------------93圖4-15、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構700℃退火(a)Cu層(b)TiWN阻障層EDS能譜圖--------------------------------95圖4-16、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-10%N2)800℃退火(c)Cu層(d)TiWN阻障層EDS能譜圖--------------------------------96圖4-17、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)as-depositedTiWN阻障層EDS能譜圖-----------------------------------97圖4-18、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)650℃退火TiWN阻障層EDS能譜圖-----------------------------------97圖4-19、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)700℃退火(a)Cu層(b)TiWN阻障層EDS能譜圖--------------------------------98圖4-20、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)800℃退火(a)Cu層(b)TiWN阻障層EDS能譜圖--------------------------------99圖4-21、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-30%N2)800℃退火(a)Cu層(b)TiWN阻障層EDS能譜圖-------------------------------100表附1-1、TiW阻障層隨溫度變化與的d值的關係--------------------114表附1-2、TiWN Ar-10N2阻障層隨溫度變化與的d值的關係-----------115表附1-3、TiWN Ar-16.6N2阻障層隨溫度變化與的d值的關係---------116表附1-4、TiWN Ar-30N2阻障層隨溫度變化與的d值的關係-----------117表附1-5、Cu4Ti的(JCPDS)相關資料----------------------------118圖附1-1、氮化鎢電阻值與濺鍍過程氮含量的關係圖----------------119圖附1-2、氮化鉭電阻值與濺鍍過程氮流量的關係圖----------------119圖附1-3、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)as-depositedTiWN層之W AES Motage圖------------------------------120圖附1-4、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)as-depositedTiWN層之N_Ti AES Motage圖--------------------------120圖附1-5、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)650℃退火TiWN層之W AES Motage圖------------------------------121圖附1-6、Si3N4(20nm)/Cu(100nm)/TiWN(20nm)/SiO2(20nm)/Si結構(Ar-16.6%N2)650℃退火TiWN層之N_Ti AES Motage圖--------------------------121圖附1-7、(Ti-Cu)二元相圖------------------------------------122 | |
dc.identifier.citation |
參考文獻1.P. J. Ding and W. A. Lanford, “Oxidation resistant high conductivity copper films, ” Appl. Phys. Lett., 64, 2897 (1994).2.W. A. Lanford, P. J. Ding, Wei Wang, S. Hymes, S. P. Murarka, “Alloying of copper for use in microelectronic metallization, ” Mater. Chem. Phys., 41, 192 (1995).3.S. D. Brotherton, J. R. Ayres, and A. Gill, H. W. van Kestern and F. J. A. M. Greidanus, “Deep levels of copper in silicon, ” J. Appl. Phys., 662, 1826(1987).4.R. N. Hall and H. Racette, J. Appl. Phys., 35, 379 (1964).5.T. Zundel, J. Weber, B. Benson, P. O. Hahn, “Ultrafast diffusion of defect in indium-doped silicon introduced by chemical mechanical polishing, ” Appl. Phys. Lett., 53, 1426 (1988).6.W. Wang, J. Foster, N. Zimmerman, A. Wendt, J. H. Booske and N. Hershkowitz, “Magnetic field rf inductively coupled argon Plasma for ionized sputtering of Cu, ” In Advanced Metallization and Interconnect Systems for ULSI Applications, 1997.7.C. Wenel, N. Urbansky, W. Klimes, and P. Siemroth, “Gap Filling with PVD process for copper metallized intergated circuited, ” Microelectric Engineering, 33, 31 (1997).8.P. Doppelt and T. H. Baum, “Chemical vapor deposition of copper for IC metallization: precursor chemistry and molecular structure, ” MRS Bulletin, 41, June 1994.9.Pascal Doppelt and Thomas H. Baum, “The chemical vapor deposition of copper and copper alloys, ” Thin Solid Film, 270, 480 (1995).10.R. J. Contolini, L. Tarte, R. T. Graff, and L. B. Evans, “Copper electroplating process for sub-half-micron ULSI structures, ” IEEE VMIC Conf, 322, 1995.11.C. W. Kaanta, S. G. Bombardier, W. J. Cote, W. R. Hill, G. Kerszykowski, H. S. Landis, D. J. Poindexter, C. W. Pollard, G. H. Ross, J. G. Ryan, S. Wolff, and J. E. Cromin, “Dual Damascene: a ULSI wring technology, ” IEEE VMIC Conf, 144 (1991).12. J. M. Sterigerwald, S. P. Murarka, R. J. Gutmann, and D. J. Duquette, “Chemical process in the chemical mechanical polishing of copper, ” Mater. Chem. Phys., 41. 217 (1995).13.Solid state Technology Apirl 2001 Vol. 44, No. 4, 30-36. (www.solid-state .com)14.M. -A. Nicolet, “Diffusion barrier in thin film, ” Thin Sold Films, 52, 415-443 (1978).15.James W. Mayer, S. S. Lau, “ Electronic materials sience:for intergrated circuits in Si and GaAs, ” 329.16.Shyam P. Murarka and Steven W.Hymes, Critical Reviews in Solid State and Materials Science, 20 (2), 87-124 (1995).17.H. Ono, T. Nakano, T. Ohta, “Diffusion barrier effects of transition metals for Cu/M/Si multi layers (M=Cr, Ti, Nb, Mo, Ta, W), ” Appl. Phys. Lett., 64, 1511 (1994).18.J. O. Olowolafe, J. Li, J. W. Mayer, and E. G. Colgan, “Effects of oxygen in TiNx on the diffusion of Cu in Cu/TiN/Al and Cu/TiNx/Si structures, ” Appl. Phys. Lett., 58, 469 (1991).19.D. -H. Kim, S. -L. Cho, K. -B. Kim, J. -J. Kim, J. -W. Park, and J. -J. Kim, “Diffusion barrier performance of chemically vapor deposited TiN films prepared using tetrakis-dimethyl-amino titanium in the Cu/TiN/Si structure, ” Appl. Phys. Lett., 69, 4182 (1996).20.Shi-Qing Wang, I. Raaijmarkers, B. J. Burrow, S. Suthar, S. Redkar, and K. -B. Kim, “Reacively sputtered TiN as a diffusion barrier between Cu and Si, ” J. Appl. Phys., 68, 5176 (1990).21.Momtchil Stavrev, Dirk Fischer, .Momtchil Stavrev, Dirk Fischer, Frank Praessler, Christian Wenzel and Kurt Drescher, “Behavior of thin Ta- based films in the Cu/barrier/Si system, ” J. Vac. Sci. Technol., A 17(3), May/Jun 1999.22.Wang MT, Lin YC, Chen MC, “Barrier properties of very thin Ta and TaN layers against copper diffusion, ” J. Electrochemi. Soci., 145, 2538(1998).23.E. Kolawa, J. S. Chen, J. S. Reid, P. J. Pokela, and M. -A. Nicolet, “Tantalum-based diffusion barriers in Si/Cu VLSI metallizations, ” J. Appl. Phys., 70, 1369 (1991).24.S. -Y. Jang, S. -M. Lee, H. K. Balk, “Tantalum and niobium as a diffusion barrier between copper and silicon, ” J. Mate. Scie., : Materials in Electronics, 7, 271 (1996).25.K. -W. Kwon, H. j. Lee, C. Ryu, R. Sinclair, and S. S Wong, “Characteristics of Ta as an underlayer for Cu Interconnects, ” in Advanced Metallization and Interconnect Systems for ULSI Applications, Oct. 1997.26.M. K. Bohr Advanced Metalization for ULSI Application In 1996 XII, Mate. Rese. Soci., 3-10 (1997).27.S. P. Murarka, Microelectron. Eng. 37/38, 29 (1997). National Technology Roadmap for Semiconductor (Semiconducto Industry Association, San Jose, CA, 1994 ; 1997).28.B. Sun, T. Chiang, P. Ding, and B. Chin, “PVD Ta and TaNx diffusion barriers and deposition techniques for copper metallization, ” Conference Proceedings ULSI XIII, 1998.29.Karen Holloway, P. M. Fryer, C. Cabral Jr, J. M. E. Harper, P. J. Bailey, and K. H. Kelleher, “Tantalum as a diffusion barrier between copper and silicon: failure mechanism and effect of nitrogen additions, ”J. Appl. Phys., 71, 5433 (1992).30.M. Stavrev, C. Wenzel, A. Moller, K. Drescher, “Sputter of tantalum-based diffusion barriers in Si/Cu metallization: effects of gas pressure and composition, ” Appl. Sur. Sci., 91, 257 (1995).31.Takeo Oku, E. Kawakami, M. Uekubo, K. Takahiro, S. Yamaguchi, M. Murakami, “Diffusion barrier property of TaN between Si and Cu, ” Appl. Sur. Sci., 99, 265, (1996).32.M.Takeyama, A. Noya, T. Sase, A. Ohta, and K. Sasaki, “Properties of TaNx films as diffusion barriers in the thermally stable Cu/Si contact systems, ” J. Vac. Sci. Technol., B, 14, 674 (1996).33.Kyung-Hoon Min, Kyu-Chang Chun, and Ki-Bum Kim, “Comparative study of tantalum and tantalum nitrides (Ta2N and TaN) as a diffusion barrier for Cu metallization, ” J. Vac. Sci. Technol., B, 14, 3263 (1996).34.J. S. Reid, E. Kolawa, R. P. Ruiz, and M. -A. Nicolet, “Evaluation of amorphous (Mo,Ta,W)-Si-N diffusion barriers for /Cu metallizations, ” Thin Solid Films, 236, 319 (1993).35.Dong Joon Kim and Yong Tae Kim, “Nanostructured Ta-Si-N diffusion barriers for Cu metallization, ” J. Appl. Phys., 82, 4847, (1997).36.E. Blanquet, A. M. Dutron, V. Ghetta, C. Bernard, R. Madar, “Evaluation of LPCVD Me-Si-N (Me=Ta, Ti, W, Re) diffusion barriers for Cu metallizations, ” Microelectronic Engineering, 37/38, 189 (1997).37.Yoon-Jik Lee, B. -S. Suh, M. S. Kwon, and C. -O. Park, “Barrier properties and failure mechanism of Ta-Si-N thin films for Cu interconnection, ”J. Appl. Phys., 85, 1927 (1999).38.T. Oku, M. Uekubo, E. Kawakami, K. Nii, T. Nakano, T. Ohta, and M. Murakami, “Thermal stability of WNx and TaNx diffusion barriers between Si and Cu, ” IEEE VMIC Conf., 182 (1995).39.Masaki Uekubo, T. Oku, K. Nii, M. Murakami, K. Takahiro, S. Yamaguchi, T. Nakano, T. Ohta, “WNx diffusion barriers between Si and Cu, ” Thin Solid Film, 286, 170-175 (1996).40.J. P. Lu, Q. Z. Hong, W. Y. Hsu, G. A. Dixit, V. Cordasco, S. W. Rusell, J. D. Lutttner, R. H. Havemann, L. K. Magel, and H. L. Tsai, “An ammonia-free PECVD process for depositing tungsten nitride films and its application in copper metallization, ” in Advanced Metallization and Interconnect Systems for Applications, Oct. 1997.41.J. R. Reid, R.Y. Liu, Paul Matrin Smith, R. P. Ruiz, M. -A Nicolet, “W-B-N diffusion barrier for Si/Cu metalization, ” Thin Solid Film, 262, 218-223 (1995).42.J. D. Luttner, R. H. Havemann, L. K. Magel, and H. L.Tasi, “An ammonia-free PECVD process for depositing tungsten nitride films and it’s application in copper metalization, ” in Advance Metalization and Interconnect Systems for ULSI Application, Oct. 1997.43.X. Sun, J. S. Reid, E. Kolawa, M. A. Nicolet, “Reactively sputtered Ti-Si-N film I. Physical properties, ” J. Appl. Phys., 81, 656 (1997).44.S. -Q. Wang, S. Suthar, C. Hoeflich, and B. J. Burrow, “Diffusion barrier properties of TiW between Si and Cu, ” J. of Appl. Phys, 73, 2301 (1993).45.J. O. Olowolafe, C. J. Mogab and R. B. Gregory, “Evaluation of Ta, Ti and TiW encapsulation for corrosion and diffusion protection of Cu interconnects, ” Thin Solid Films, 227, 37-43 (1993).46.B. R. Rogers, C. J. Tracy and T. S. Cale, “Compositional variation In sputtered Ti-W films due to re-emission, ” J. Vac. Sci. Technol., B 12 (5), Sep/Oct.47.Do-Heyoung Kim, Robert H. Wentorf, Jr., and William N. Gill, “Nucleation of copper on TiW and TiN during chemical deposition, ”J. Appl. Phys., 74 (8), 15 October 1993.48.Akira Furuya, Nobuki Hosoi, and Yoshio Ohshita, “Evaluation of Cu adhesive energy on barrier metals by means of contact-angle measurement, ” J. Appl. Phy., 78 (10), 15 Movember 1995.49.David R. Evans and David M. Leet, “3%Ti–Tungsten Diffusion Barriers, ”J. Electrochem. Soc., Vol. 141, No. 7, July 1994.50.Jung-Chao Chiou, Kuen-Chi Juang, and Mao-Chieh Chen, “TiW(N) as Diffusion Barrier between Cu and Si, ” J. Electrochem. Soc., Vol. 142, No. 7, July 1995.51.Fukada, T.; Mori.; Toyoda, Y.; Hasegawa, M.; Namba, K.; Ogata, K.,“Electromigration resistance of TiWN/Cu/TiWN interconnections, ”Applied Surface Science, Volume:91, October, 227-233,1995.52.J. H. Moser, F. Tian, O. Haller, D. B. Bergstrom, I. Pertov, J. E. Greene, C. Wiemer, “Single-phase polycrystalline Ti1-xWxN Alloys (0≦x≦0.7) grown by UHV reactive magnetron sputtering:microstructure and physical properties, ” Thin Solid Films, 253, 445-450 (1994).53.Eric Cheney, Dennis Lazaroff, hewlett-packard, Corvallis, Oregn, Diana Morales, Lip Yap, Leon Chiu, Johnson Matthey Electronics, Spokane, Washington, “Defect performance for PVD of TiW and TiWN films, ” Solid State Technology, Nivember, 109-114 (1997).54.H. Ramarotafika and G. Lemperiere, “Influence of a d. c. substrate bias on the resistivity, composition, crystallite size and microstrain of WTi and WTi-N films, ” Thin Solid Films, 266, 267-273 (1995).55.T. Hurkmans, T. Trinh, D. B. Lewis, J. S. Brooks and W. -D. Munz, ”Multiayered titanium tungsten nitride coatings with a superlattice structure grown by unbalanced magnetron sputtering,” Surface and CoatingTechnology 76-77, 159-166 (1995).56.J. M. Oparowski, R. D. Sisson, Jr., and R. R. Biederman, “The parameters on the microstructure and properties of sputter-desposited TiW thin film Diffusion barriers, ” Thin Solid Films, 153, 313-328 (1987).57.A. G. Dirk, R. A. M. Wolters and A. J. Nellissien, “On the Microstructure-property relationship of W-Ti-(N) Diffusion barriers, ” Thin Solid Films, 193/194, 201-210 (1990).58.K. S. Weil, J. Y. Kim, P. N. Kumta, “Synthesis of nanoscale titanium nitride - tungsten nitride alloy powders using a novel complexed precursor, ” Mate. Lett., 39, 292-297 (1999).59.Mayumi Takeyama, Atsushi Noya, and Tomoyuki Fukda, “Thermal stability of Cu/W/Si contact system using layer of Cu(111) and W(110) perferred orientations, ” J. Vac. Sci. technol., A 15(2), Mar/Apr 1997.60.Ivo J. Raaijmakers, Tarshish Setalvad, Ameet S. Bhansali, Bard J. Burrow, Laslo Gutai and Ki-Bum Kim, “Microstructure and Barrier Properties of Reactively Sputtered Ti-W Nitride, ” J. Elec. Mate., 19, 1221-1226 (1990).61.A. S. Bhansali, I. J. M. M. Raaijmakers, R. Sinclair, A. E. Morgan, B. J.Burrow and M. Arst, “A Phase Diagram Approach For Predicting Reactions In Al/TiW(-Nitride) Thin-Film Systems, ” Material Research Society Symp. Proc. Vol. 187, 15-20 (1990).62.Frank C. T. So, Elzbieta, Kolawa, Xin-An Zhao and Marc-A. Nicolet, “WNx : Properties and Application, ” Thin Solid Films, 153, 507-520 (1987).63.Bong-Seok Suh, Yoon-Jik Lee, Jeong-Sug Hwang, Chong-Ook Park, “ Properties of reactively sputtered WNx as Cu diffusion barrier, ” Thin Solid Films, 384, 299-303 (1999).64.L. Boukhris, J. -M. Poitevin, “Electrical resistivity, structure and composition of d.c. sputtered WNx films, ” Thin Solid Films, 310, 222-227 (1997).65.J. R. Lloyd and J. J. Clement, Microelectric Engineering, Vol. 31,P.41.66.L. B Jonsson, C. Hedlund, I. V. Katardjiev, S. Berg, “Comopsitional variations of sputter deposited Ti/W barrier layer on substrate with pronounced surface topography, ” Thin Solid Films, 348, 227-232 (1999).67.V. G. Glebovsky, V. Yu. Yaschak, V. V. Baranov, E. L. Sackovich, “Properties of titanium-tungsten thin films obtained by magnetron sputtering of composite cast trgets, ” Thin Solid Films, 257, 1-6 (1995).68.J. Dunlop, E. Waterman and T. Brat, “Effect of Ti-W target processing method on defect generation during very large scale Integrated device fabrication, ” J. Vac. Sci. Technol. A 10 (2), Mar/Apr, 305-312 (1992).69.R. A. M. Wolters and A. J. M. Nellissen, “Properties of Reactive Sputtered TiW, ” Solid State Technology/February, 131-136 (1996 ).70.Michael Hill, “Magnetron Sputterde Titanium-Tungsten Films, ”Solid State Technology/January, 53-59 (1980).71.Jiang, ET AI., Solid State Technology, Vol. 42, No. 4, 1999.72.H. Ono, T. NaKano, and T. Ohta, Appl. Phys. Lett., 64 (12), 1511-1513 (1994).73.Dong Joon Kim, Young Tae Kim, and John Wan Park, J. Vac. Sci. Tenchnol., B, 17 (4), 1598-1601 (1999).74.G. Bai, S.Wittenbrock, V. Ochoa, R. Villasol, C. Chiang, T. Marieb, D. Gardner, C. Mu, D. Fraser, and M. Bohr, “Effectiveness and reliability of metal diffusion barrier for copper interconnects, ” MRS Symp. Proc., 403, 501 (1996).75.Sa-Kyun Rha, W. -J. Lee, S. -Y, Lee, D. -W. Kim, C. -O. Park, S. -S. Chun, “ interdiffusion and reactions in Cu/TiN/Ti/Si and Cu/TiN/Ti/SiO2/Si multilayer structures, ” J. Mate. Rese., 12, 3367 (1997).76.L. C. Lane, T. C. Nason, G. -R. Yang, T. -M. Lu, and H. Bakhru, “ Secondary ion mass spectrometry study of thermal stability of Cu/refractory metal/Si structures, ” J. Appl. Phys., 69, 6719 (1991).77.Chung-Shi, and Lih-Juann Chen, “ Interfacial Reactions of Copper Thin Films on Silicon and Materials Issues of Cu Metallization in ULSI Devices, ” 國立清華大學材料科學研究所,博士論文, 民國八十四年六月二十四日, 117-128頁.78.S. Josson, “Reevaluation of the Ti-W System and Prediction of the Ti-W-NPhase Diagram, ” Carl Hanser Verlag, Munchen Z. Metallkd, 87, 10, 784-787 (1996).79.Y. T. Kim, C. H. Jun, and D. Y. Kim, Thin Solid Films, 347, 214 (1999).80.J. J. Guo, and G.S.Chen, “Evaluation of Radio-Frequency Sputtered TexturedTiN Thin films as Diffusion Barriers between Copper and Silicon, ”真空科技 十三卷一期, 4-13頁.81.G. S. Chen, P. Y. Lee and S. T. Chen, “Pfase formation behavior and diffusion barrier property of reactively sputtered tantalum-based thin films used in semiconductormetallization, ” Thin Solid Film, 353,264-273 (1999). | |
dc.identifier.uri |
https://hdl.handle.net/20.500.14371/20249 | |
dc.language.iso |
中文 | |
dc.relation.alma |
990008926960206772 | |
dc.relation.page |
122 | |
dc.subject.keyword |
鎢化鈦 | |
dc.subject.keyword |
鈦鎢氮化物 | |
dc.subject.keyword |
銅 | |
dc.subject.keyword |
擴散阻障層 | |
dc.subject.keyword |
TiW | |
dc.subject.keyword |
TiWN | |
dc.subject.keyword |
Cu | |
dc.subject.keyword |
Diffusion barrier | |
dc.title |
鎢化鈦與鈦鎢氮化物薄膜應用於銅金屬化之擴散阻障層特性研究 | zh-TW |
dc.title |
Diffusion barrier layer properties of TiW and TiWNthin films in copper metallization system | en |
dc.type |
Thesis | zh-TW |
檔案
本條目沒有附加檔案。
所屬典藏: 材料科學與工程學系