利用金屬鈍化層技術優化低溫銅對銅接合之熱穩定性並探討接合面之微結構對可靠度之影響
Enhancement of Thermal Stability in Low-temperature Cu-Cu Bonding by Metal Passivation Layer and Investigation of Interface Microstructure Impact on Reliability
摘要
本論文旨在研究利用金屬鈍化層技術優化銅對銅接合結構的熱穩定性及可靠性,並分析退火過程中接合結構內部機制的影響。透過臨場穿透式電子顯微鏡(In-situ TEM)觀察退火過程中接合介面的即時變化,探討不同接合結構的退火機制。對於退火過程中的接合品質變化,進行不同退火時間的機械強度測試和電性表現的比較。最後,探討可靠性測試前後特徵接觸電阻的變化,進而確認鈍化層應用在銅對銅接合中的潛力。
本研究比較含鈍化層以及無鈍化層的銅對銅接合結構在180 ℃下的臨場退火行為,選擇的鈍化層材料包含3 nm APC以及Thin film Ag (TF-Ag)。過往的研究已分析鈍化層結構之接合機制,其接合介面形貌主要分為兩種: 銅原子擴散區域和鈍化層直接接合區域。In-situ TEM的臨場退火分析結果顯示,3 nm APC鈍化層結構在鈍化層直接接合區域呈現團簇聚集的現象,而TF-Ag鈍化層結構維持穩定的狀態。在銅原子擴散區域,兩種鈍化層結構則一致呈現結晶化以及接合介面消弭現象。X射線光電子能譜(XPS)和TEM分析顯示,鈍化層直接接合區域的退火機制差異與鈍化層的擴散速率有關,TF-Ag的擴散速率較快,APC較慢,導致APC鈍化層結構的接合介面保留較多銀原子,進而形成團簇現象。此外,透過4D-STEM應力分析確認,鈍化層材料的擴散是透過銅晶界進行。對於無鈍化層的銅對銅接合結構,在180 ℃臨場退火過程中觀察到孔洞成核及孔洞成長現象,導致接合品質劣化。
在180 ℃退火條件下,透過拉力測試和Kelvin structure電性測量,評估含鈍化層以及無鈍化層之銅對銅接合結構的接合品質之熱穩定性。結果顯示,TF-Ag和APC鈍化層結構的接合品質均優於無鈍化層的銅對銅接合結構,與臨場分析的結果相同。值得注意的是,兩種鈍化層結構在退火過程中的電性趨勢不同: TF-Ag的電阻值持續上升,而APC則呈現先下降後上升,這是由於銅和銀的電阻率差異以及兩種鈍化層材料擴散速度不同所致。
由於在180 ℃退火下含鈍化層以及無鈍化層的銅對銅接合結構僅顯示微觀結構變化,因此進一步進行300 ℃高溫退火測試。結果顯示,無鈍化層之銅對銅接合結構出現異常晶粒成長、大量孔洞形成及去雙晶現象,而TF-Ag和APC鈍化層結構無明顯孔洞。這些差異源於鈍化層材料沿銅晶界的擴散,導致晶界偏析強化現象,進一步增強鈍化層結構的熱穩定性。此外,300 ℃退火後的電性測量結果顯示,兩種鈍化層結構的電阻值均優於無鈍化層之銅對銅接合結構,顯示出鈍化層結構具備優良的熱穩定性。由此可知,鈍化層在銅對銅接合中不僅保護銅表面,還作為熱穩定劑的角色。
30 nm APC鈍化層結構在先前的研究中已被驗證,透過增加鈍化層直接接合區域的比例能優化接合性能。在180 ℃退火過程中,其電性表現趨勢與3 nm APC鈍化層結構相似,這是由於鈍化層厚度增加導致銅擴散速度變慢,從而延遲了電阻值上升的時間。最後,3 nm和30 nm APC鈍化層結構在可靠性測試中,亦展現良好的電性性能。本論文的研究證實,鈍化層結構能夠改善接合結構的熱穩定性,並保持優良的可靠性表現,顯示出其在先進封裝產業中的應用前景。
本研究比較含鈍化層以及無鈍化層的銅對銅接合結構在180 ℃下的臨場退火行為,選擇的鈍化層材料包含3 nm APC以及Thin film Ag (TF-Ag)。過往的研究已分析鈍化層結構之接合機制,其接合介面形貌主要分為兩種: 銅原子擴散區域和鈍化層直接接合區域。In-situ TEM的臨場退火分析結果顯示,3 nm APC鈍化層結構在鈍化層直接接合區域呈現團簇聚集的現象,而TF-Ag鈍化層結構維持穩定的狀態。在銅原子擴散區域,兩種鈍化層結構則一致呈現結晶化以及接合介面消弭現象。X射線光電子能譜(XPS)和TEM分析顯示,鈍化層直接接合區域的退火機制差異與鈍化層的擴散速率有關,TF-Ag的擴散速率較快,APC較慢,導致APC鈍化層結構的接合介面保留較多銀原子,進而形成團簇現象。此外,透過4D-STEM應力分析確認,鈍化層材料的擴散是透過銅晶界進行。對於無鈍化層的銅對銅接合結構,在180 ℃臨場退火過程中觀察到孔洞成核及孔洞成長現象,導致接合品質劣化。
在180 ℃退火條件下,透過拉力測試和Kelvin structure電性測量,評估含鈍化層以及無鈍化層之銅對銅接合結構的接合品質之熱穩定性。結果顯示,TF-Ag和APC鈍化層結構的接合品質均優於無鈍化層的銅對銅接合結構,與臨場分析的結果相同。值得注意的是,兩種鈍化層結構在退火過程中的電性趨勢不同: TF-Ag的電阻值持續上升,而APC則呈現先下降後上升,這是由於銅和銀的電阻率差異以及兩種鈍化層材料擴散速度不同所致。
由於在180 ℃退火下含鈍化層以及無鈍化層的銅對銅接合結構僅顯示微觀結構變化,因此進一步進行300 ℃高溫退火測試。結果顯示,無鈍化層之銅對銅接合結構出現異常晶粒成長、大量孔洞形成及去雙晶現象,而TF-Ag和APC鈍化層結構無明顯孔洞。這些差異源於鈍化層材料沿銅晶界的擴散,導致晶界偏析強化現象,進一步增強鈍化層結構的熱穩定性。此外,300 ℃退火後的電性測量結果顯示,兩種鈍化層結構的電阻值均優於無鈍化層之銅對銅接合結構,顯示出鈍化層結構具備優良的熱穩定性。由此可知,鈍化層在銅對銅接合中不僅保護銅表面,還作為熱穩定劑的角色。
30 nm APC鈍化層結構在先前的研究中已被驗證,透過增加鈍化層直接接合區域的比例能優化接合性能。在180 ℃退火過程中,其電性表現趨勢與3 nm APC鈍化層結構相似,這是由於鈍化層厚度增加導致銅擴散速度變慢,從而延遲了電阻值上升的時間。最後,3 nm和30 nm APC鈍化層結構在可靠性測試中,亦展現良好的電性性能。本論文的研究證實,鈍化層結構能夠改善接合結構的熱穩定性,並保持優良的可靠性表現,顯示出其在先進封裝產業中的應用前景。
This thesis aims to investigate the optimization of thermal stability and reliability in Cu-Cu bonding structures using metal passivation layer technology, and analyze the effects of annealing processes on the internal mechanisms of bonding structures. Real-time observations using in-situ TEM study the annealing mechanisms of different bonding structures. Changes in bonding quality during annealing are compared through mechanical strength tests and electrical performance assessments. Finally, variations in specific contact resistance before and after reliability testing are analyzed to confirm the potential of passivation layers.
The study compares the in-situ annealing behavior of Cu-Cu bonding structures with and without passivation layers at 180 ℃. The passivation materials selected include 3 nm APC and thin film Ag (TF-Ag). Previous studies have analyzed the bonding mechanisms of passivation structures and have shown that the bonding interface morphology mainly consists of two regions: The Cu atoms diffusion region and the passivation direct bonding region. In-situ TEM analysis indicates that the 3 nm APC passivation structure exhibits agglomeration in the passivation direct bonding region, whereas the TF-Ag passivation structure remains stable. In the Cu atom diffusion region, both passivation structures consistently exhibit crystallization and the vanishing of the bonding interface. XPS and TEM analyses reveal that the differences in annealing mechanisms in the passivation direct bonding region are related to the diffusion rates of the passivation layers, with TF-Ag diffusing faster than APC, leading to the retention of more Ag atoms at the bonding interface in the APC passivation structure, forming agglomeration. Furthermore, stress mapping via 4D-STEM confirms that passivation interdiffusion occurs through Cu grain boundaries. For Cu-Cu bonding structures without passivation layers, void nucleation and growth are observed during in-situ annealing at 180 ℃, leading to a deterioration in bonding quality during prolonged annealing.
The thermal stability of Cu-Cu bonding structures with and without passivation layers under 180 ℃ annealing conditions is evaluated through pull tests and electrical measurements using a Kelvin structure. Results show that the bonding quality of the TF-Ag and APC passivation structures is superior to that of the Cu-Cu bonding structures without passivation layers, consistent with in-situ analysis results. Notably, the electrical performance trends of the two passivation structures differ during annealing: the electrical resistance of TF-Ag continuously increases, whereas that of APC initially decreases and then increases. This difference is attributed to variations in the resistivity of Cu and Ag and the different diffusion rates of the passivation materials.
Since the Cu-Cu bonding structures with and without passivation layers show only microscopic structural changes at 180 ℃ annealing, further high-temperature annealing at 300 ℃ is conducted. Results indicate that the Cu-Cu bonding structures without passivation layers exhibit abnormal grain growth, extensive void formation, and de-twinning, whereas the TF-Ag and APC passivation structures show no significant voids. These differences are due to the diffusion of passivation materials along Cu grain boundaries, leading to grain boundary segregation strengthening, which further enhances the thermal stability of the passivation structures. Additionally, electrical measurements after 300 ℃ annealing show that the electrical resistance of the two passivation structures is superior to that of the Cu-Cu bonding without passivation layers, demonstrating good thermal stability of Cu-Cu bonding with passivation layers. Therefore, passivation layers in Cu-Cu bonding not only protect the Cu surface but also act as thermal stabilizers.
Previous studies have demonstrated that the 30 nm APC passivation structure optimizes bonding performance by increasing the proportion of the passivation direct bonding region. During 180 ℃ annealing, its electrical performance trend is similar to that of the 3 nm APC passivation structure, as the increased thickness of the passivation layer slows the diffusion rate of Cu, thereby delaying the rise in resistance. Finally, the 3 nm and 30 nm APC passivation structures also exhibit good electrical performance in further reliability testing. Overall, these passivation structures exhibit greater thermal stability and achieve lower bonding temperatures than the Cu-Cu direct bonding structure, highlighting the potential of passivation layer technology for advanced electronic devices.
The study compares the in-situ annealing behavior of Cu-Cu bonding structures with and without passivation layers at 180 ℃. The passivation materials selected include 3 nm APC and thin film Ag (TF-Ag). Previous studies have analyzed the bonding mechanisms of passivation structures and have shown that the bonding interface morphology mainly consists of two regions: The Cu atoms diffusion region and the passivation direct bonding region. In-situ TEM analysis indicates that the 3 nm APC passivation structure exhibits agglomeration in the passivation direct bonding region, whereas the TF-Ag passivation structure remains stable. In the Cu atom diffusion region, both passivation structures consistently exhibit crystallization and the vanishing of the bonding interface. XPS and TEM analyses reveal that the differences in annealing mechanisms in the passivation direct bonding region are related to the diffusion rates of the passivation layers, with TF-Ag diffusing faster than APC, leading to the retention of more Ag atoms at the bonding interface in the APC passivation structure, forming agglomeration. Furthermore, stress mapping via 4D-STEM confirms that passivation interdiffusion occurs through Cu grain boundaries. For Cu-Cu bonding structures without passivation layers, void nucleation and growth are observed during in-situ annealing at 180 ℃, leading to a deterioration in bonding quality during prolonged annealing.
The thermal stability of Cu-Cu bonding structures with and without passivation layers under 180 ℃ annealing conditions is evaluated through pull tests and electrical measurements using a Kelvin structure. Results show that the bonding quality of the TF-Ag and APC passivation structures is superior to that of the Cu-Cu bonding structures without passivation layers, consistent with in-situ analysis results. Notably, the electrical performance trends of the two passivation structures differ during annealing: the electrical resistance of TF-Ag continuously increases, whereas that of APC initially decreases and then increases. This difference is attributed to variations in the resistivity of Cu and Ag and the different diffusion rates of the passivation materials.
Since the Cu-Cu bonding structures with and without passivation layers show only microscopic structural changes at 180 ℃ annealing, further high-temperature annealing at 300 ℃ is conducted. Results indicate that the Cu-Cu bonding structures without passivation layers exhibit abnormal grain growth, extensive void formation, and de-twinning, whereas the TF-Ag and APC passivation structures show no significant voids. These differences are due to the diffusion of passivation materials along Cu grain boundaries, leading to grain boundary segregation strengthening, which further enhances the thermal stability of the passivation structures. Additionally, electrical measurements after 300 ℃ annealing show that the electrical resistance of the two passivation structures is superior to that of the Cu-Cu bonding without passivation layers, demonstrating good thermal stability of Cu-Cu bonding with passivation layers. Therefore, passivation layers in Cu-Cu bonding not only protect the Cu surface but also act as thermal stabilizers.
Previous studies have demonstrated that the 30 nm APC passivation structure optimizes bonding performance by increasing the proportion of the passivation direct bonding region. During 180 ℃ annealing, its electrical performance trend is similar to that of the 3 nm APC passivation structure, as the increased thickness of the passivation layer slows the diffusion rate of Cu, thereby delaying the rise in resistance. Finally, the 3 nm and 30 nm APC passivation structures also exhibit good electrical performance in further reliability testing. Overall, these passivation structures exhibit greater thermal stability and achieve lower bonding temperatures than the Cu-Cu direct bonding structure, highlighting the potential of passivation layer technology for advanced electronic devices.
所屬典藏
電子研究所引用此條目
Lin, T.-Y. (2024). Enhancement of Thermal Stability in Low-temperature Cu-Cu Bonding by Metal Passivation Layer and Investigation of Interface Microstructure Impact on Reliability. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/3064
引用文字依 APA 第 7 版格式自動產生,使用前請再核對。
分享
永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/3064