移除齒顎矯正支架後之牙釉質破壞分析

Failure analysis of enamel after removing orthodontic bracket

檔案

日期

2005

類型

語言

中文

摘要

由於近年來齒顎矯正技術的進步,大部份齒列不整與異常咬合不正之病患仍然施以矯正器方式進行齒顎矯正治療。黏著在牙釉質上之齒顎矯正支架(bracket)為齒顎矯正方法之重要裝置。當矯正完成後,使用各式不同施力方式的支架移除工具移除齒顎矯正支架時,輕則會造成黏著劑殘留齒面問題,重則會有發生牙釉質損傷的可能。所以本研究目的為探討矯正支架的移除負荷模式與牙釉質損傷情形,以及瞭解齒面上黏著劑殘留量情形。
為進行牙釉質損傷與黏著劑殘留程度的分析與評估,本研究透過材料試驗機進行體外試驗,包括拉力、剪力與扭力試驗,將拉力與剪力之移除速度設定為1㎜/min,扭力之移除速度設定為10°/min,分別對已處理完畢之試片做材料試驗,以求得真實力量輸出。接著,把所有試驗完畢之試片及矯正支架放置在掃描式電子顯微鏡下紀錄觀測齒面破壞情形,兩者互相對照,以找出不同施力負荷與支架-黏著劑-牙釉質間之關聯性。最後,利用影像分析軟體Optimas 6.5 進行影像分析,在影像中框選出牙釉質損傷及黏著劑殘留面積與中心位置,藉以針對牙釉質破壞及黏著劑殘留做定量及定性之分析。另外,將已知的矯正支架底部面積繪製成一3×3 矩陣之圖形,把影像分析後所得到的牙釉質損傷與黏著劑殘留及矯正支架底部空洞中心位置皆填入矩陣圖形中,以清楚瞭解齒面上之破壞位置。
研究結果指出在拉力試驗結果的平均負荷值為58.1 ± 39.9 N,可得到5.9MPa的平均拉應力。在剪力試驗結果的平均負荷值為79.9 ± 53.6 N,可得到8.1MPa的平均剪應力。在扭力試驗結果的平均負荷值為159.5 ± 98.9 N-mm。從齒面破壞影像與影像分析結果可得知,在拉力試驗中,有3 顆試片發現牙釉質損傷,損傷位置大致座落於咬合、齒齦、近心、遠心側的角落部位。黏著劑殘留面積總量為72.8mm2,平均黏著劑殘留面積為7.28mm2(74%)與牙釉質損傷面積總量為0.57mm2,平均牙釉質損傷面積為0.06mm2。而最大拉力負荷為133N,造成最大的牙釉質損傷量為2.7%與最少的黏著劑殘留量41%。在剪力試驗中,有4 顆試片發現牙釉質損傷,損傷位置大致座落於近心側部位。黏著劑殘留面積總量為36.95mm2,平均黏著劑殘留面積為3.7mm2(37%)與牙釉質損傷面積總量為1.38mm2,平均牙釉質損傷面積為0.14mm2。而最大剪力負荷為168N,造成最大的牙釉質損傷量為5.7%與極少黏著劑殘留量為12%。在扭力試驗中,有6 顆試片發現牙釉質損傷,損傷位置大致座落於咬合側與齒齦側的角落部位。黏著劑殘留面積總量為50.49mm2,平均黏著劑殘留面積為5.05mm2(51%)與牙釉質損傷面積總量為2.64mm2,平均牙釉質損傷面積為0.27mm2。而最大扭力負荷為345N-mm,造成最大的牙釉質損傷量為7.8%與極少的黏著劑殘留量為15%。
研究結果顯示施力負荷越大,牙釉質損傷面積就越大,黏著劑殘留面積也越小,齒面破壞位置座落於黏著劑與牙釉質間的機會就越高,而且在施力端的位置較容易出現牙釉質損傷的情形。從影像分析結果可得知,扭力負荷在移除支架過後對於牙釉質會有嚴重損傷的趨勢,且大部份試片的破壞層面均介於黏著劑和牙釉質之間。另外,在拉力與剪力負荷方面,對於齒面上牙釉質損傷及黏著劑殘留面積,兩負荷間則無太大之差異。
Since the orthodontic technology has been improved in recent years,the greater part of tooth alignment disorder and malocclusion patients used orthodontic bracket to proceed orthodontic treatment. Orthodontic bracket bonded to etched enamel is a very important appliance. When the
treatment is finished, orthodontic bracket often used different loading modes to debond. If adhesive residual remains on the enamel, finishing procedures are required. However, it’s possible to damage enamel when clear the adhesive residual. Moreover, the enamel has been fractured
when debonding orthodontic bracket. The purpose of this study is to analyze the relationship between the loading modes of debonding bracket and the enamel damages, as well as to understand adhesive residual remaining on the enamel.
To analyze enamel fracture and adhesive residual, all specimens were bonded to the bracket and then be assessed at a universal material testing machine. These specimens were respectively subjected to a tensile force and shear force at a crosshead speed of 1 mm/min, and torque at a
crosshead speed of 10°/min. After debonded the brackets, all specimens were inspected under the SEM (Scanning Electron Microscope) to record the enamel fractured and bracket base cavities. All specimens images were analyzed by the image software Optimas 6.5, including the enamel
fractured area and adhesive residual area.
This study indicated that the debonding loads were the 58.1±39.9N at tensile modes, the 79.9±53.6N at shear modes and 159.5±98.9N-mm at torsion modes. The average shear stress and tensile stress were respectively estimated to 5.9 and 8.1 MPa. Under a tensile mode, the three specimens were observed to enamel fracture located at corners. The
maximum tensile force reached 133N, which exhibited the greatest enamel fracture occupied 2.7% of total area and the least adhesive residual occupied 41% of total area. Under a shear mode, the four specimens were observed to enamel fracture located at right side. The maximum shear force reached 168N, which exhibited the greatest enamel
fracture occupied 5.7% of total area and the least adhesive residual capacity was 12% of total area. Under a torsion mode, the six specimens were observed to enamel fracture located near corners. The maximum torque reached 345N-mm, which exhibited the greatest enamel fracture occupied 7.8% of total area and the least adhesive residual occupied 15%of total area.
This study indicated a trend existed in that the more debonding force would result in more enamel fracture and less adhesive residual. Additionally, its failure surface was occurred between adhesive and enamel. As to the enamel damage, this study didn’t suggest the torsion mode to debond bracket since it was possible to fracture more enamel.However, the shear and tensile model to debond bracket had no remarkable discrepancy about enamel fracture and adhesive residual.
顯示完整詮釋資料 統計資料

引用此條目

陳柄廷 (2005). 移除齒顎矯正支架後之牙釉質破壞分析. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/32808

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/32808