摘要

纖維蛋白(FN)及透明質酸( hyaluronate,HA)在傷口癒合時扮演細胞模板及提供細胞訊號的功能。為了充分利用此二高分子調控生理的功能,本研究以還原胺法偶合短鏈HA(short chain hyaluronate,sHA)及纖維蛋白原,合成新的分子複合體,並將此纖維蛋白原/短鏈透明質酸”複合物定性。
三個不同接枝比的偶合物(sHA-g-fibrinogens),其上平均所接枝的sHA個數分別為2.22、4.82及6.59,分別將其稱為S2.2F、S4.8F 及 S6.6F,此三個比例的偶合物仍保留纖維蛋白原可凝膠的特性。纖維蛋白(FN)、S2.2F、 S4.8F 及 S6.6F所導出之纖維直徑分別約為117 nm、149 nm、359 nm 及 399 nm。經由凝膠通透性測量可得偶合物之達西係數,其值分為7.77±1.39 cm2(FN) 、11.00±1.12cm2(S2.2F) 、 93.03±14.98cm2(S4.8F)及439.7±100.1cm2(S6.6F)。由以上之數據可知纖維直徑及凝膠通透性於S2.2F與S4.8F之間有一巨大的轉變。
偶合物之黏著強度(Adhesion strength)隨著接枝比的增加而減小,其值由大而小分別為FN (2.21±0.20N)> S2.2F (1.62±0.11N)> S4.8F (1.03±0.09N)> S6.6F (0.62±0.12N)。而在另一方面,偶合物凝膠之水含量隨著接枝比上升而增加,大小依序為FN (31.72 ±0.12%)> S2.2F(33.45 ±0.09%)> S4.8F(37.80 ±0.35%)> S6.6F(39.96 ±0.73%)。F、S2.2F、 S4.8F 及 S6.6F之凝膠時間(lag period of the fibrin gelling)分別為11min、14min、15.5min及16.5min,而最終黏度依序為14.18 cp (FN) 、11.39cp F(S2.2F)、9.35 cp(S4.8F)、7.57 cp(S6.6F)。
由研究結果可知,經由改變sHA的進料比可得到不同接枝比的偶合物,所合成出之偶合物於性質上已有別於纖維蛋白(FN) ,但仍保留纖維蛋白可凝膠之特性。故於未來之應用上,可利用此新方法,依照用途之不同,合成適當接枝比之偶合物與之應用。
Fibrinogen (FN) and hyaluronic acid (HA) are both key components of cellular signal cascade and of the template for cell growth during the process of wound healing. In order to fully utilize the physiological functions of these two molecules, we have synthesized a new molecular hybrid by grafting sHA (short-chain HA) to fibrinogen molecule via the reducing-end coupling of sHA with the amino groups of fibrinogen. The resulted sHA-g-fibrinogen molecules were characterized in this study.
Three different sHA-g-fibrinogens coupled with average sHA molecules of 2.22, 4.82 and 6.59 were synthesized and designated as S2.2F, S2.8F and S6.6F, respectively. All three sHA-g-fibrinogens retained the gelling ability similar to fibrinogen. The diameters of the fibrin fibrils derived from fibrinogen (FN), S2.2F, S4.8F and S6.6F were estimated to be about 117 nm, 149 nm, 359 nm and 399 nm, respectively. The values of Darcy constants obtained from permeability test are 7.77±1.39 cm2 (F), 11.00±1.12cm2 (S2.2F), 93.03±14.98cm2 (S4.8F) and 439.7±100.1cm2 (S6.6F). Both of the fibril diameter and the permeability of the fibrin network changed drastically between S2.2F and S4.8F.
The adhesion strengths changed inversely to the graft ratio; i.e., FN (2.21±0.20N) > S2.2F (1.62±0.11N) >S4.8F (1.03±0.09N) > S6.6F (0.62±0.12N). On the other hand, the water content of the fibrin gel increased with increasing graft ratio; FN (31.72 ±0.12%)>S2.2F(33.45 ±0.09%)>S4.8F(37.80 ±0.35%)>S6.6F(39.96 ±0.73%). The lag periods of the fibrin gelling of FN, S2.2F, S4.8F and S6.6F were 11min, 14min, 15.5min and 16.5min, respectively, with the resulted viscosities of 14.18 cp (F), 11.39cp (S2.2F), 9.35 cp (S4.8F) and 7.57 cp (S6.6F).
The current study indicates that a series of sHA-g-fibrinogens can be prepared by varying the graft ratio of sHA to fibrinogen. All of these fibrinogen derivatives retained the gelling capability but with different fibrin gel properties. By use of our new approach, specific fibrinogen derivative can be tailor-made to meet the specific need of fibrin glue for future application.
顯示完整詮釋資料 統計資料

引用此條目

周芝伶 (2005). 纖維蛋白原與短鏈透明質酸偶合物之合成與定性. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/33004

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/33004