摘要

隨著現今高功率元件需求提高,提供晶片與基板間連接散熱的熱界面材料(TIM)選擇因此漸趨重要,本研究選用具高導熱係數的銅作為熱壓接合的材料。為了使 TIM 適應粗糙度的問題,實驗中以銅鋅共電鍍後去合金的方式取得奈米孔洞銅(NP-Cu),孔隙率約15%、孔徑 40 nm,且調整電鍍條件以加強結構與基板的接著。此外結構中也加入高<111>優選方向的奈米雙晶銅(NT-Cu),以實現銅-銅於更低溫度下接合並提升機械強度。
當 NP-Cu 或 NT-Cu 作為接合中間層時,於 250℃、30 分鐘、30 MPa 下,機械強度超過 17 MPa,且 NP-Cu 能使界面成功接合的面積提高。 當使用 NT-Cu 時,接合溫度能降低至 200℃且機械強度為 10.35 MPa。當濺鍍 NT-Cu 之碳化矽基板接合電鍍 NP-Cu 的銅基板時,於 250℃、30 分鐘、30 MPa 接合條件下能達到幾乎無縫隙之界面,且爐冷後的機械強度為 17.27 MPa。若銅基板改為覆銅陶瓷基板,僅 15 分鐘接合後的結構可通過1000 循環之溫度循環測試,且接合界面良好具一定可靠度。此外 NP-Cu 的導熱係數為293.3 W/(mK)。從不同的接合結果得知降伏強度低的 NP-Cu 能透過形變減低粗糙度的影響,而高<111>優選方向的 NT-Cu 能降低接合溫度並提升機械性質,因此透過兩者的結合,能取得高導熱係數及良好可靠度的接合結構,提供適用於高功率元件封裝中的 TIM。
With the increasing demand for high-power devices, ensuring a robust connection between the chip and the substrate, while providing efficient heat dissipation, has become crucial. To address the issue of high operating temperatures and the insufficient thermal conductivity of TIMs in power devices, Cu was selected, and thermal compression bonding method was used in this study. Firstly, to overcome the roughness between the TIM and substrates, a nanoporous copper (NP-Cu) structure was fabricated through dealloying after Cu/Zn co-electroplating. The porosity and pore size of the structure was about 15% and 40 nm. Electroplating conditions were optimized to improve the adhesion between NP-Cu and the substrate. Additionally, highly <111>-oriented nanotwinned copper (NT-Cu) was applied to enhance the bonding quality and reduce bonding temperature.
The results show that under 250°C, 30 minutes, and 30 MPa, when NP-Cu or NT-Cu was used as an interlayer, mechanical strength can exceed 17 MPa. The existence of NP-Cu can further increase the bonding fraction. When NP-Cu was bonded to NT-Cu, the bonding temperature can lower to 200°C with a strength of 10.35 MPa. Furthermore, SiC can be bonded to rough copper substrates with the aid of NP-Cu and NT-Cu. The bonding strength is 17.27 MPa with almost no seams at the interface. When NT-Cu and NP-Cu are used to bond SiC and ceramic substrate, after 15 minutes of bonding, the structure can pass 1000 thermal cycles demonstrating a good reliability. Also, the thermal conductivity of NP-Cu was tested as 293.3 W/(mK). The combination of NT-Cu and NP-Cu results in high thermal conductivity and good reliability, making it a promising TIM in high-power device packaging.
顯示完整詮釋資料 統計資料

引用此條目

盧琬心 (2024). 奈米孔洞銅與<111>方向奈米雙晶銅箔應用於熱界面材料接合之高功率元件封裝研究. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/3559

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/3559