利用噴霧乾燥包覆氧化還原石墨烯技術及多孔二氧化矽薄膜生長法應用在雙核-殼結構純矽負極之改良研究
Enhanced Pure Silicon Anode with Dual Core-Shell Structure Using Reduced Graphene Oxide Coating and Porous Silica Thin Film via Spray Drying
摘要
Silicon anode-based lithium-ion batteries (LIBs) suffer from severe capacity degradation due to volume expansion and fracturing caused by the formation of the Li15Si4 alloy during charging and discharging. To address this, we employed a dual-coating technique using spray-dried reduced graphene oxide (rGO) and tetraethyl orthosilicate (TEOS) as the precursor for the silicon dioxide (SiO2) film to design the electrode structure.
First, we investigated the impact of rGO and TEOS coatings in different positions on the electrode and identified the optimal configuration as Si@TEOS@rGO. We found that Si55@TEOS29@rGO16, with 29% TEOS, showed the best cycling performance. After determining the optimal dual-coating condition, we compared the effects of adding 0.5wt%, 1wt%, and 2wt% of TMSPi and TEOS as electrolyte additives. Results revealed that Si55@TEOS29@rGO16 with 1wt% TMSPi exhibited the best cycle life.
Additionally, we used TEOS as a precursor for the SiO2 film through the Stöber method sol-gel process, forming a porous SiO2 film on Si particles (Si@TEOS) using CTAB as an organic growth template. This film created an artificial SEI layer of lithium silicates during lithiation, controlling silicon expansion, improving ion conductivity, and preventing direct contact between the electrolyte and the silicon electrode. We then coated the Si@TEOS with graphene oxide (GO) via spray drying and thermally reduced it at 950°C in an Ar atmosphere to form Si@TEOS@rGO. This rGO layer absorbed expansion stress, prevented direct electrolyte contact, and increased conductivity between particles.
Finally, the Si55@TEOS29@rGO16+1wt% TMSPi electrode showed an average capacity decay of only 4.8% per cycle after 300 cycles at 0.5C, compared to 12.4% per cycle for pure Si, marking an improvement of over 2.5 times. This confirms the effectiveness of our structural design in mitigating capacity degradation in silicon-based anodes.
First, we investigated the impact of rGO and TEOS coatings in different positions on the electrode and identified the optimal configuration as Si@TEOS@rGO. We found that Si55@TEOS29@rGO16, with 29% TEOS, showed the best cycling performance. After determining the optimal dual-coating condition, we compared the effects of adding 0.5wt%, 1wt%, and 2wt% of TMSPi and TEOS as electrolyte additives. Results revealed that Si55@TEOS29@rGO16 with 1wt% TMSPi exhibited the best cycle life.
Additionally, we used TEOS as a precursor for the SiO2 film through the Stöber method sol-gel process, forming a porous SiO2 film on Si particles (Si@TEOS) using CTAB as an organic growth template. This film created an artificial SEI layer of lithium silicates during lithiation, controlling silicon expansion, improving ion conductivity, and preventing direct contact between the electrolyte and the silicon electrode. We then coated the Si@TEOS with graphene oxide (GO) via spray drying and thermally reduced it at 950°C in an Ar atmosphere to form Si@TEOS@rGO. This rGO layer absorbed expansion stress, prevented direct electrolyte contact, and increased conductivity between particles.
Finally, the Si55@TEOS29@rGO16+1wt% TMSPi electrode showed an average capacity decay of only 4.8% per cycle after 300 cycles at 0.5C, compared to 12.4% per cycle for pure Si, marking an improvement of over 2.5 times. This confirms the effectiveness of our structural design in mitigating capacity degradation in silicon-based anodes.
矽陽極組成的鋰離子電池(LIBs)因充放電過程中Li15Si4合金的形成引起的體積膨脹、碎裂,導致嚴重的容量衰減。為了改善這一問題,本研究採取了噴霧乾燥rGO包覆技術以及TEOS作為二氧化矽薄膜前驅物的雙重包覆對電極結構進行設計。首先,我們探討了rGO和TEOS包覆在不同位置對於電極的影響,並找出最佳位置為Si@TEOS@rGO。接著,我們進一步研究最佳TEOS添加比例,結果顯示TEOS佔29%的Si55@TEOS29@rGO16在循環性能方面表現最佳。在確定最佳雙殼層包覆條件為Si55@TEOS29@rGO16後,我們又比較了添加0.5wt%、1wt%和2wt% TMSPi和TEOS作為電解液添加劑,最終發現1wt% TMSPi條件下的Si55@TEOS29@rGO16具有最好的循環壽命。
此外,本研究使用TEOS作為二氧化矽薄膜的前驅物,通過Stöber method溶膠-凝膠法讓TEOS在乙醇溶劑中用氨當作催化劑和水反應,並以CTAB作為有機生長模板,在Si顆粒上生成多孔二氧化矽薄膜(Si@TEOS)。這層多孔且具剛性的SiO2薄膜在鋰化反應中,會形成矽酸鋰的人工SEI層,能有效抑制矽的膨脹、提高離子傳導效率,並防止電解液與矽電極直接接觸,從而避免劇烈、不均勻的SEI層生長。另外,我們通過噴霧乾燥包覆氧化石墨烯(GO)在Si@TEOS上,並在Ar氣氛下以950°C熱還原形成Si@TEOS@rGO。這層rGO不僅能吸收膨脹應力,還能阻隔電解液直接接觸,並增加顆粒之間的導電度。
最終,所獲得的Si55@TEOS29@rGO16+1wt%TMSPi在定電流0.5C的充放電循環中,在300圈循環後每個循環的容量衰減平均僅為4.8%,相較於Si每個循環的容量衰減平均為12.4%提高了超過2.5倍,證明了本研究結構設計對緩解基於矽的陽極容量衰減的有效性。
此外,本研究使用TEOS作為二氧化矽薄膜的前驅物,通過Stöber method溶膠-凝膠法讓TEOS在乙醇溶劑中用氨當作催化劑和水反應,並以CTAB作為有機生長模板,在Si顆粒上生成多孔二氧化矽薄膜(Si@TEOS)。這層多孔且具剛性的SiO2薄膜在鋰化反應中,會形成矽酸鋰的人工SEI層,能有效抑制矽的膨脹、提高離子傳導效率,並防止電解液與矽電極直接接觸,從而避免劇烈、不均勻的SEI層生長。另外,我們通過噴霧乾燥包覆氧化石墨烯(GO)在Si@TEOS上,並在Ar氣氛下以950°C熱還原形成Si@TEOS@rGO。這層rGO不僅能吸收膨脹應力,還能阻隔電解液直接接觸,並增加顆粒之間的導電度。
最終,所獲得的Si55@TEOS29@rGO16+1wt%TMSPi在定電流0.5C的充放電循環中,在300圈循環後每個循環的容量衰減平均僅為4.8%,相較於Si每個循環的容量衰減平均為12.4%提高了超過2.5倍,證明了本研究結構設計對緩解基於矽的陽極容量衰減的有效性。