摘要

塑膠製品與我們的生活息息相關,然而由於環境保護的思潮日漸提升導致傳統的石化塑膠逐漸被淘汰。聚乳酸與奈米纖維素作為生質材料,皆具有優秀的材料性能,作為複合材料則更能相互補強,並展現出極大的發展價值。然而至目前為止,針對奈米纖維素強化聚乳酸的製備方法都需要耗費不少的能源耗損或製程時間。
本研究的目的在於利用工業上最常見的單螺桿射出成型機,以物理方式將纖維素解纖,並使纖維分散於聚乳酸內,製備出奈米纖維素-聚乳酸複合材料,並探討製程中的參數變化對於複合材料力學性質造成的影響。
本研究以材料的表面改質與否、加熱參數、螺桿轉速、材料擠製次數等作為操作變因,觀察纖維在聚乳酸中的解纖效率和分佈情形,並探討不同的操作變因對於複合材料的射出成型品強度帶來的影響。
研究結果顯示,隨著材料擠製次數的提升,複合材料中會有越多的纖維被解纖成奈米纖維,直至直徑均一的奈米纖維素在基材中交錯排列;纖維的水熱改質是將纖維束解纖成奈米纖維的必要條件,在未改質下的纖維不論如何進行擠製製程皆會維持在微米直徑大小;增加螺桿轉速與製程溫度能提升纖維的解纖效率,使纖維更快被分解成奈米纖維素。
於拉伸試驗分析結果中,與純聚乳酸材料相比,未改質纖維的複合材料提升抗拉強度32.5%,而經表面改質的複合材料提升抗拉強度55.3%,證實本研究之複合材料製備方法能夠對材料強度有所提升。
Plastic products are closely related to our daily lives, but as environmental protection awareness increases, traditional petrochemical plastics are gradually being phased out. Polylactic acid (PLA) and nanocellulose, as biobased materials, exhibit excellent material properties and, when used as composite materials, can complement each other and demonstrate significant development potential. However, up to now, the methods for preparing nanocellulose-reinforced PLA typically require considerable energy consumption or processing time.
The aim of this study is to use the most commonly used single-screw injection molding machine in industry to physically fibrillate cellulose and disperse the fibers within PLA to produce nanocellulose-PLA composite materials. The study also investigates the impact of process parameters on the mechanical properties of the composite material.
This study explores the effects of surface modification of materials, heating parameters, screw rotation speed, and extrusion frequency as operational variables. It observes the efficiency of fiber fibrillation and distribution in PLA, and examines how different operational variables affect the strength of the injection-molded composite products.
According to the research results, with increasing extrusion frequency, more fibers in the composite material are fibrillated into nanocellulose, resulting in uniformly sized nanocellulose fibers interspersed within the matrix. Hydrothermal modification of fibers is essential for fibrillating fiber bundles into nanocellulose; unmodified fibers, regardless of extrusion processing, remain at the micron size. Increasing screw rotation speed and processing temperature can enhance the fibrillation efficiency, leading to faster decomposition of fibers into nanocellulose.
In tensile tests, composites with unmodified fibers show a 32.5% increase in tensile strength compared to pure PLA materials, while composites with surface-modified fibers show a 55.3% increase in tensile strength. This confirms that the composite material preparation method in this study can enhance the strength of the material.

所屬典藏

機械工程學系
顯示完整詮釋資料 統計資料

引用此條目

翁齊甫 (2024). 以單螺桿擠製機製備奈米纖維素-聚乳酸複合材料:針對纖維素解纖效率與複合材料的機械性質進行探討. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/3979

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/3979