開發用於應力感知的環氧基預聚物與力學響應型三唑啉二酮衍生物
Development of Epoxy-based Prepolymers for Stress-Sensing and a Triazolinedione-based Mechanophore
摘要
In modern materials science, it has become possible to introduce mechanophores into polymer materials, leading to the development of mechanoresponsive materials. Such materials have the unique ability to visualize damage, preventing unforeseen mishaps during usage.
In this study, we successfully devised a method to introduce mechanophores into epoxy materials, using spiropyran derivatives. Employing atom transfer radical polymerization, we connected epoxy moieties to spiropyran derivatives. Subsequently, we obtained epoxy materials containing mechanophores by combining spiropyran with epoxy groups, polyamine as a crosslinker, and through a thermal crosslinking process. Moreover, we subjected these materials to scratch and puncture tests to confirm their mechanical responsiveness.
Besides, we synthesized a novel mechanophore, a Diels-Alder adduct (TAD-An), composed of 4,4'-(4,4'-diphenylmethane)-bis(1,2,4-triazine-3,5-dione) (MDI-TAD) and anthracene. This mechanophore can be incorporated into polymer chains, and when external forces are applied to the polymer chains, the TAD-An within the chains undergoes a retro Diels-Alder reaction at the C-N bond, inducing fluorescence from the embedded anthracene. To explore the impact of intramolecular bond energy differences on mechanical responsiveness, we synthesized a structurally similar mechanophore (MAL-An) using bismaleimide as a dienophile as a comparison, which would undergo a retro Diels-Alder reaction at the C-C bond upon mechanical stress. Subsequently, we analyzed the polymer fracture rate constants for TAD-An and MAL-An. Experimental results indicated that the polymer fracture rate constants for TAD-An (C-N bond) were 1.58642 × 10-5 min-1, while that for MAL-An (C-C bond) was 1.39630 × 10-5 min-1.
In this study, we successfully devised a method to introduce mechanophores into epoxy materials, using spiropyran derivatives. Employing atom transfer radical polymerization, we connected epoxy moieties to spiropyran derivatives. Subsequently, we obtained epoxy materials containing mechanophores by combining spiropyran with epoxy groups, polyamine as a crosslinker, and through a thermal crosslinking process. Moreover, we subjected these materials to scratch and puncture tests to confirm their mechanical responsiveness.
Besides, we synthesized a novel mechanophore, a Diels-Alder adduct (TAD-An), composed of 4,4'-(4,4'-diphenylmethane)-bis(1,2,4-triazine-3,5-dione) (MDI-TAD) and anthracene. This mechanophore can be incorporated into polymer chains, and when external forces are applied to the polymer chains, the TAD-An within the chains undergoes a retro Diels-Alder reaction at the C-N bond, inducing fluorescence from the embedded anthracene. To explore the impact of intramolecular bond energy differences on mechanical responsiveness, we synthesized a structurally similar mechanophore (MAL-An) using bismaleimide as a dienophile as a comparison, which would undergo a retro Diels-Alder reaction at the C-C bond upon mechanical stress. Subsequently, we analyzed the polymer fracture rate constants for TAD-An and MAL-An. Experimental results indicated that the polymer fracture rate constants for TAD-An (C-N bond) were 1.58642 × 10-5 min-1, while that for MAL-An (C-C bond) was 1.39630 × 10-5 min-1.
在現代的材料科學中,可以透過在高分子中引入力學響應分子 (mechanophore),得到具有機械力響應性的材料 (mechanoresponsive material)。這類材料可以使受損狀況視覺化 (visualize),有助於避免使用過程中發生意料外的災害。
在本研究中我們成功透過螺吡喃衍生物開發出一種能廣泛地將力學響應分子引入環氧材料的方法。我們透過原子轉移自由基聚合,將環氧基團連接至螺吡喃衍生物上。然後混合作為交聯劑的多元胺,通過熱交聯過程,我們成功製備出內含力學響應分子的環氧材料。接著,我們也通過划刮和穿刺測試,驗證了材料的機械力響應性。
此外,我們還合成了由4,4'-(4,4'-二苯甲基)-雙(1,2,4-三唑啉-3,5-二酮) (MDI-TAD) 和蒽構成的狄爾斯-阿爾德加成物 (Diels-Alder adduct) (TAD-An)。這種力學響應分子能夠嵌入高分子鏈中,並當外界施加力於高分子鏈時,鏈中的TAD-An在C-N鍵上會發生逆狄爾斯-阿爾德反應(retro Diels-Alder),從而讓內部的蒽產生螢光訊號。為了探究分子內的鍵能差異對於力學響應性的影響,我們以雙馬來酰亞胺 (bismaleimide) 作為二烯親和體 (dienophile) 合成了相似結構的力學響應分子 (MAL-An),此分子受力後會在C-C鍵上發生逆狄爾斯-阿爾德反應。隨後我們對TAD-An與MAL-An進行高分子斷裂速率常數的分析,實驗結果表明:TAD-An(C-N鍵)的高分子斷裂速率常數為1.58642 × 10-5 min-1,而MAL-An(C-C鍵)的高分子斷裂速率常數為1.39630 × 10-5 min-1。
在本研究中我們成功透過螺吡喃衍生物開發出一種能廣泛地將力學響應分子引入環氧材料的方法。我們透過原子轉移自由基聚合,將環氧基團連接至螺吡喃衍生物上。然後混合作為交聯劑的多元胺,通過熱交聯過程,我們成功製備出內含力學響應分子的環氧材料。接著,我們也通過划刮和穿刺測試,驗證了材料的機械力響應性。
此外,我們還合成了由4,4'-(4,4'-二苯甲基)-雙(1,2,4-三唑啉-3,5-二酮) (MDI-TAD) 和蒽構成的狄爾斯-阿爾德加成物 (Diels-Alder adduct) (TAD-An)。這種力學響應分子能夠嵌入高分子鏈中,並當外界施加力於高分子鏈時,鏈中的TAD-An在C-N鍵上會發生逆狄爾斯-阿爾德反應(retro Diels-Alder),從而讓內部的蒽產生螢光訊號。為了探究分子內的鍵能差異對於力學響應性的影響,我們以雙馬來酰亞胺 (bismaleimide) 作為二烯親和體 (dienophile) 合成了相似結構的力學響應分子 (MAL-An),此分子受力後會在C-C鍵上發生逆狄爾斯-阿爾德反應。隨後我們對TAD-An與MAL-An進行高分子斷裂速率常數的分析,實驗結果表明:TAD-An(C-N鍵)的高分子斷裂速率常數為1.58642 × 10-5 min-1,而MAL-An(C-C鍵)的高分子斷裂速率常數為1.39630 × 10-5 min-1。