4H-SiC基板之反應濺鍍TiN磊晶薄膜及其高溫退火研究
Reactive Sputtering Deposition and High-temperature Annealing of Epitaxial TiN Thin Films on 4H-SiC
摘要
透過直流磁控反應濺射沉積法在半絕緣單晶(0001) SiC基板上成功生長TiN磊晶薄膜。研究生長溫度與氮氣/氬氣之流量比,對薄膜質量及生長速率之影響。X光繞射(X-ray diffractometer, XRD)及穿透式電子顯微鏡(Transmission electron microscope, TEM)分析顯示,在550 °C和700 °C下所沉積之TiN薄膜均在SiC上磊晶成長,TiN與4H-SiC之磊晶關係為(111)TiN//(0001)SiC與[1"1" ̅0]TiN//[11"2" ̅0]4H-SiC。將氮氣流量比從4%增加到8%可改善薄膜品質並降低生長速率。於700°C下以8%流量比沉積之TiN薄膜,其TiN(111)之X-ray Rocking Curve半高寬度可達到249 arcsec,且TiN薄膜電阻率測得21 μΩ∙cm。原子力顯微鏡(Atomic force microscopy, AFM)測量顯示,TiN薄膜的表面粗糙度可以低至Rq 1.1 nm。X光電子能譜(X-ray photoelectron spectroscopy, XPS)顯示所有生長的薄膜的TiN成分均接近平衡的化學計量比。
為深入了解高溫退火對TiN薄膜品質和界面擴散現象之影響,透過感應式加熱爐對沉積之TiN薄膜於1150°C至1700 °C溫度範圍內進行退火。結果顯示TiN薄膜於1250 °C退火時,TiN(111)的半高全寬(FWHM)減少約30%。隨著退火溫度升高至1400 °C,薄膜成分逐漸富含碳,形成TiCxN1-x,且x值可達0.5。經過1700 °C退火後,薄膜進一步富含碳,x值超過0.5。利用TEM觀察與分析,薄膜長時間在1700 °C退火,將導致SiC基板分解並形成石墨、非晶碳及孔洞。
為深入了解高溫退火對TiN薄膜品質和界面擴散現象之影響,透過感應式加熱爐對沉積之TiN薄膜於1150°C至1700 °C溫度範圍內進行退火。結果顯示TiN薄膜於1250 °C退火時,TiN(111)的半高全寬(FWHM)減少約30%。隨著退火溫度升高至1400 °C,薄膜成分逐漸富含碳,形成TiCxN1-x,且x值可達0.5。經過1700 °C退火後,薄膜進一步富含碳,x值超過0.5。利用TEM觀察與分析,薄膜長時間在1700 °C退火,將導致SiC基板分解並形成石墨、非晶碳及孔洞。
Epitaxial TiN thin films were successfully grown on semi-insulating single-crystal (0001) SiC substrates using DC reactive magnetron sputtering. The effects of growth temperature and the nitrogen/argon flow ratio on the film quality and growth rate were studied. X-ray diffraction (XRD) and transmission electron microscopy (TEM) analyses revealed that TiN films deposited at 550 °C and 700 °C grew epitaxially on SiC, with the epitaxial relationship between TiN and 4H-SiC being (111)TiN //(0001)SiC and [1"1" ̅0]TiN//[11"2" ̅0]4H-SiC. Increasing the nitrogen flow ratio from 4% to 8% improved the film quality and reduced the growth rate. The TiN film deposited at 700 °C with an 8% nitrogen flow ratio exhibited an X-ray rocking curve (XRC) FWHM of 249 arcsec for TiN(111) and a resistivity of 21 μΩ∙cm. Atomic force microscopy (AFM) measurements showed that the surface roughness of the TiN film could be as low as Rq 1.1 nm. X-ray photoelectron spectroscopy (XPS) revealed that the TiN composition of all grown films was close to the stoichiometric ratio.
To further understand the effects of high-temperature annealing on the TiN film quality and interfacial diffusion phenomena, the deposited TiN films were annealed in an induction heating furnace within a temperature range of 1150 °C to 1700 °C. The results indicated that the FWHM of TiN(111) decreased by approximately 30% when annealed at 1250 °C. As the annealing temperature increased to 1400 °C, the film composition gradually became carbon-rich, forming TiCxN1-x, with x reaching up to 0.5. After annealing at 1700 °C, the film further enriched with carbon, with x exceeding 0.5. TEM observations and analyses showed that prolonged annealing at 1700 °C led to the decomposition of the SiC substrate, resulting in the formation of graphite, amorphous carbon, and voids.
To further understand the effects of high-temperature annealing on the TiN film quality and interfacial diffusion phenomena, the deposited TiN films were annealed in an induction heating furnace within a temperature range of 1150 °C to 1700 °C. The results indicated that the FWHM of TiN(111) decreased by approximately 30% when annealed at 1250 °C. As the annealing temperature increased to 1400 °C, the film composition gradually became carbon-rich, forming TiCxN1-x, with x reaching up to 0.5. After annealing at 1700 °C, the film further enriched with carbon, with x exceeding 0.5. TEM observations and analyses showed that prolonged annealing at 1700 °C led to the decomposition of the SiC substrate, resulting in the formation of graphite, amorphous carbon, and voids.