旋轉鈦輪電鍍奈米雙晶銅箔的強化方法與解決強度-延展性(導電率)折衷問題的途徑
Strengthening Methods of Rotary-Electroplated Nanotwinned Copper Foils and Approaches to Resolve the Strength-Ductility (Electrical Conductivity) Trade-Off
摘要
為了提高電子產品的品質和可靠度,銅箔應具有適當的強度以抵抗機械失效、足夠的延展性以便於成型和提供撓性,優異的導電性以提高信號傳輸效率,以及足夠的薄度以增加能量密度和減輕重量。通過使用添加劑,奈米雙晶能夠藉由直流電旋轉電鍍系統生成於銅箔當中,該製程與實際電鍍銅箔的生產過程高度類似。低濃度的銅離子或高含量的添加劑可以提高強度,但會減少延展性(或導電性)。因此,本研究探討並討論了進一步增強奈米雙晶銅箔而不降低其延展性和導電性的方法,並將銅箔的厚度控制在15-20微米。
通過引入鈷離子和降低電鍍溫度,解決了強度與延展性(或導電性)之間的困境。這兩種強化方法的結合在保持延展性和導電性的同時,使得抗拉強度 (UTS)和降伏強度(YS)分別提高了21% 和13%,達到866 MPa的抗拉強度和640 MPa的降伏強度。
另外,通過調整電流密度,合成了具有晶粒尺寸和雙晶間距梯度的雙層 (2L) 和三層 (3L) 異質銅箔。三層異質銅箔,由於界面數量較多和顯著的結構梯度,顯示出明顯提高的強度和加工硬化率,同時展現了延長的斷裂伸長率。這歸因於表面強化、更多的幾何必要差排生成以及被有效抑制的軟質區域內塑性應變。
通過引入鈷離子和降低電鍍溫度,解決了強度與延展性(或導電性)之間的困境。這兩種強化方法的結合在保持延展性和導電性的同時,使得抗拉強度 (UTS)和降伏強度(YS)分別提高了21% 和13%,達到866 MPa的抗拉強度和640 MPa的降伏強度。
另外,通過調整電流密度,合成了具有晶粒尺寸和雙晶間距梯度的雙層 (2L) 和三層 (3L) 異質銅箔。三層異質銅箔,由於界面數量較多和顯著的結構梯度,顯示出明顯提高的強度和加工硬化率,同時展現了延長的斷裂伸長率。這歸因於表面強化、更多的幾何必要差排生成以及被有效抑制的軟質區域內塑性應變。
To improve the quality and reliability of electronic products, the Cu foils should be equipped with appropriate strength to resist mechanical failure, sufficient ductility for shaping and flexibility, excellent electrical conductivity to increase signal transmission efficiency, and thinness for energy density and lightweight. With the use of additives, nano twins are generated in the Cu foils by the rotary electrodeposition system using a direct current that is highly analogous to the actual manufacturing process of electroplated Cu foils. A low concentration of Cu ions or a high content of additives resulted in enhanced strength but undermined ductility (or electrical conductivity). Accordingly, methods to further strengthen nanotwinned Cu foils without reducing ductility and electrical conductivity were explored and discussed in this study, and the thickness of Cu foils was controlled at 15-20 μm.
The breakthrough of the dilemma between strength and ductility (or electrical conductivity) was found by the involvement of Co ions and the low plating temperature. Maintaining ductility and conductivity, the combination of these two strengthening methods increased the ultimate tensile strength (UTS) and yield strength (YS) by 21% and 13%, respectively, with UTS of 866 MPa and YS of 640 MPa. In addition, by tuning the current density, the two-layered (2L) and three-layered (3L) heterogeneous Cu foils were synthesized with gradients in the grain size and twin spacing. 3L types, with more interfaces and significant structural gradients, exhibited obvious advancement in strength and work hardening rate and showed extended elongation to failure, which was attributed to surface strengthening, motivated formation of geometrically necessary dislocations, and efficient suppression of plastic strain in the soft part.
The breakthrough of the dilemma between strength and ductility (or electrical conductivity) was found by the involvement of Co ions and the low plating temperature. Maintaining ductility and conductivity, the combination of these two strengthening methods increased the ultimate tensile strength (UTS) and yield strength (YS) by 21% and 13%, respectively, with UTS of 866 MPa and YS of 640 MPa. In addition, by tuning the current density, the two-layered (2L) and three-layered (3L) heterogeneous Cu foils were synthesized with gradients in the grain size and twin spacing. 3L types, with more interfaces and significant structural gradients, exhibited obvious advancement in strength and work hardening rate and showed extended elongation to failure, which was attributed to surface strengthening, motivated formation of geometrically necessary dislocations, and efficient suppression of plastic strain in the soft part.
所屬典藏
材料科學與工程學系引用此條目
Hung, Y.-W. (2024). Strengthening Methods of Rotary-Electroplated Nanotwinned Copper Foils and Approaches to Resolve the Strength-Ductility (Electrical Conductivity) Trade-Off. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/4523
引用文字依 APA 第 7 版格式自動產生,使用前請再核對。
分享
永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/4523