三維積體電路中接合淺碟孔洞的演化

Evolution of Dishing Voids in the Cu-Cu Bonding for 3DIC

檔案

全文未公開。

日期

2023

類型

語言

中文

摘要

隨著科技的進步,電子產品的傳輸及儲存能力需求增加並追求輕薄短小,使用外導線作為連接方法的二維封裝已不敷使用。為了延續摩爾定律,三維積體電路(3D-IC)技術應運而生,利用矽穿孔(Through Silicon Via)將晶片垂直堆疊並接合,以降低晶片封裝體積及提升電晶體密度。銅因其優異的物理特性和成本效益成為主要的接合材料。在接合之前,通常會使用化學機械研磨(CMP)處理晶片表面以達到平坦化,然而研磨過程可能導致淺碟現象,這會影響接合強度和元件性能。本實驗以無優選方位的電鍍銅和帶有淺碟的電鍍銅柱進行接合,在不同溫度下進行熱壓接合,並進行加壓與不加壓的退火處理。最後使用聚焦離子束顯微鏡(FIB)觀察接合介面的拋光情況,探討淺碟造成的孔洞在熱壓和退火過程中的變化。
通過比較孔洞高度、接合比率和孔洞比率等指標,可以了解接合結果並探討孔洞演變的機制。研究結果顯示,不同溫度下的加壓退火可以逐漸修復孔洞,並且在特定條件下(例如長時間於200℃或短時間於250℃和300℃)可以成功實現接合,並透過不加壓力退火觀察在一小時至二十四小時接合介面劣化情形,以確保接合後的介面品質和元件可靠性。
With the constant advancement of technology, the pursuit of high-speed computing, large-capacity memory, and lightweight and compact electronic devices has become a trend. To perpetuate Moore's Law, the technology of Three-Dimensional Integrated Circuits (3D-IC) has emerged, which involves vertically stacking and bonding chips using Through Silicon Vias (TSVs). Copper has become the main bonding material due to its excellent physical properties and cost efficiency. Before bonding, the chip surfaces are typically subjected to Chemical Mechanical Polishing (CMP) for planarization. However, the polishing process may lead to dishing, which can affect bonding strength and device performance. In this experiment, bonding was performed using randomly oriented electroplated copper and electroplated copper pillars with dishing. Bonding was conducted at different temperatures, followed by annealing with and without applied pressure. The polished interfaces were observed using Focused Ion Beam (FIB) to examine the changes in dishing-induced voids during the bonding and annealing processes. By comparing indicators such as void height, bonding ratio, and void ratio, the bonding results and the evolution mechanism of voids can be understood. The research results showed that annealing with applied pressure at different temperatures gradually repaired the voids, and successful bonding was achieved under specific conditions (e.g., long duration at 200 °C or short duration at 250 °C and 300 °C). Non-pressure annealing was also conducted for one to twenty-four hours to observe the degradation of the bonding interface, thereby verifying the reliability of the devices. With the development of technology, vertically integrated 3D- ICs have significant application value in lightweight, compact electronic devices. However, the issue of dishing on copper surfaces still needs to be addressed to ensure the quality of the bonded interface and device reliability.
顯示完整詮釋資料 統計資料

引用此條目

黃凱翔 (2023). 三維積體電路中接合淺碟孔洞的演化. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/519

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/519