A chitosan/iridium/sodium hyaluronate (CHI-Ir-SH) composite scaffold with an unique
honeycomb-like microstructure is fabricated via electrophoretic deposition (EPD). Due to the
formation of hydrogen bubbles during EPD process, the scaffold deposited on the working
electrode contains vertical pore channels arranged in a honeycomb-like configuration. The
diameter and length of the pore channels are 230.3 μm and 230.1 μm, respectively. The scaffold
exhibits a porosity of 76.7% and an impressive water uptake of 350%. With the addition of
iridium, the tensile strength for the scaffold is almost doubled to 8.7 MPa, as compared to the
counterpart without the addition of iridium. For the scaffold, the iridium nanoparticles are
homogeneously distributed with an average size of 8.4 nm. The predominance of metallic
iridium instead of Ir3+ or Ir4+ ions suggests that the iridium nanoparticles are chelated stably
within the scaffold. For cell migration test, the relative migration of 122% compared with
control group for HaCaT cells in the scaffold indicates a promising wound healing ability.
honeycomb-like microstructure is fabricated via electrophoretic deposition (EPD). Due to the
formation of hydrogen bubbles during EPD process, the scaffold deposited on the working
electrode contains vertical pore channels arranged in a honeycomb-like configuration. The
diameter and length of the pore channels are 230.3 μm and 230.1 μm, respectively. The scaffold
exhibits a porosity of 76.7% and an impressive water uptake of 350%. With the addition of
iridium, the tensile strength for the scaffold is almost doubled to 8.7 MPa, as compared to the
counterpart without the addition of iridium. For the scaffold, the iridium nanoparticles are
homogeneously distributed with an average size of 8.4 nm. The predominance of metallic
iridium instead of Ir3+ or Ir4+ ions suggests that the iridium nanoparticles are chelated stably
within the scaffold. For cell migration test, the relative migration of 122% compared with
control group for HaCaT cells in the scaffold indicates a promising wound healing ability.
透過電泳沉積這個製程,我們成功地製備了具特殊蜂巢狀結構的幾丁聚醣/銥/玻尿
酸鈉複合膜,當薄膜沉積於工作電極上時,氫氣氣泡的產生佔據了薄膜可沉積的位置,
使得薄膜內部構成了直通微孔結構,而透過測量,這些直通微孔的直徑為 230.3 微米、
長度為 230.1 微米,正是這些密集排列的直通孔結構使得我們的薄膜具有 76.7 %的孔隙
率以及 350 %的吸水量。此外,和不添加銥的薄膜相比,透過添加銥可以讓倍增我們薄
膜的拉伸強度至 8.7 MPa,且這些銥還會均勻地在我們的薄膜內形成銥奈米粒子,其平
均大小為 8.4 奈米。而透過儀器測量,我們發現薄膜內部的銥主要以零價的金屬態存於
其中,而非氧化過後的三價或四價態,這點說明了幾丁聚醣和添加的銥螯合在一起並穩
定的存於薄膜內。而人類皮膚角質細胞(HaCaT cells)的相對遷移率則近一步驗證了我們
薄膜是具有傷口修復效果的,其數值可達 122%。而上述這些性質讓我們製備出的薄膜
在生醫領域上有潛在的應用。
酸鈉複合膜,當薄膜沉積於工作電極上時,氫氣氣泡的產生佔據了薄膜可沉積的位置,
使得薄膜內部構成了直通微孔結構,而透過測量,這些直通微孔的直徑為 230.3 微米、
長度為 230.1 微米,正是這些密集排列的直通孔結構使得我們的薄膜具有 76.7 %的孔隙
率以及 350 %的吸水量。此外,和不添加銥的薄膜相比,透過添加銥可以讓倍增我們薄
膜的拉伸強度至 8.7 MPa,且這些銥還會均勻地在我們的薄膜內形成銥奈米粒子,其平
均大小為 8.4 奈米。而透過儀器測量,我們發現薄膜內部的銥主要以零價的金屬態存於
其中,而非氧化過後的三價或四價態,這點說明了幾丁聚醣和添加的銥螯合在一起並穩
定的存於薄膜內。而人類皮膚角質細胞(HaCaT cells)的相對遷移率則近一步驗證了我們
薄膜是具有傷口修復效果的,其數值可達 122%。而上述這些性質讓我們製備出的薄膜
在生醫領域上有潛在的應用。
所屬典藏
材料科學與工程學系引用此條目
Chen, L.-J. (2023). Fabrication of chitosan/iridium/sodium hyaluronate composite scaffold with honeycomb-like microstructure and its wound healing ability. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/616
引用文字依 APA 第 7 版格式自動產生,使用前請再核對。
分享
永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/616