摘要
本論文主要探討以微波電漿氮化(100)矽晶片上之TiO2薄膜,所形成之磊晶TiN薄膜,則做為緩衝層,以微波電漿化學氣相沉積法(MPCVD)沉積鑽石薄膜於矽晶片基板,並分析其晶向分布。論文第一部分主要探討微波電漿氮化法的製程參數對氮化TiO2之影響,藉由不同的氫氣濃度、微波功率、微波時間及總壓力,以得到品質較佳之TiN薄膜層。第二部分則藉由不同偏壓條件及成長時間來成長鑽石薄膜,並探討鑽石成長在TiN/Si(100)之特徵。
在TiN製程部分,藉由微波電漿氮化法,以通入氮氣與氫氣之混合氣體將50 nm 厚之TiO2薄膜氮化為TiN,藉由不同的氫氣濃度、微波功率、總製程時間及總製程壓力來控制TiN的晶體方向性及其結晶品質。分析技術方面,應用掃描式電子顯微鏡(SEM)來觀察表面形貌;X光繞射儀(XRD)和X光光電子能譜儀(XPS)分析結構相與化學組成;穿透式電子顯微鏡(TEM)分析TiN與矽基板界面的關係。TiN磊晶品質與氫氣濃度和微波功率有關,氫氣濃度從0.4%增加至4%,則有助於形成TiN磊晶,700W的微波功率及50 torr的壓力能夠得到較佳的TiN薄膜,結晶品質從X-ray rocking curve (XRC) 可得約為0.199之半高寬。
在鑽石薄膜成長在TiN/Si之研究,則嘗試以不同偏壓及成長時間等製程參數成長鑽石膜,比較這兩者對鑽石膜成長之影響。利用SEM、Raman光譜儀對鑽石膜做表面形貌及鍵結情形的分析,以TEM分析鑽石、TiN、矽基板三者之間的界面情形,並對方向性鑽石膜成長的可能性做分析和討論。結果發現偏壓成核階段,形成多晶鑽石奈米晶粒之鑽石及其他非晶碳於TiN之上,成核密度超過1.5 x 109 cm-2;成長階段可形成具有方向性之鑽石。
在TiN製程部分,藉由微波電漿氮化法,以通入氮氣與氫氣之混合氣體將50 nm 厚之TiO2薄膜氮化為TiN,藉由不同的氫氣濃度、微波功率、總製程時間及總製程壓力來控制TiN的晶體方向性及其結晶品質。分析技術方面,應用掃描式電子顯微鏡(SEM)來觀察表面形貌;X光繞射儀(XRD)和X光光電子能譜儀(XPS)分析結構相與化學組成;穿透式電子顯微鏡(TEM)分析TiN與矽基板界面的關係。TiN磊晶品質與氫氣濃度和微波功率有關,氫氣濃度從0.4%增加至4%,則有助於形成TiN磊晶,700W的微波功率及50 torr的壓力能夠得到較佳的TiN薄膜,結晶品質從X-ray rocking curve (XRC) 可得約為0.199之半高寬。
在鑽石薄膜成長在TiN/Si之研究,則嘗試以不同偏壓及成長時間等製程參數成長鑽石膜,比較這兩者對鑽石膜成長之影響。利用SEM、Raman光譜儀對鑽石膜做表面形貌及鍵結情形的分析,以TEM分析鑽石、TiN、矽基板三者之間的界面情形,並對方向性鑽石膜成長的可能性做分析和討論。結果發現偏壓成核階段,形成多晶鑽石奈米晶粒之鑽石及其他非晶碳於TiN之上,成核密度超過1.5 x 109 cm-2;成長階段可形成具有方向性之鑽石。
This thesis focuses on the study of diamond film growth on Si substrate using a TiN buffer layer formed by plasma nitriding of TiO2 based on the microwave plasma technology of (MPCVD). The effect of various plasma nitriding conditions on the formation of TiN was firstly explored to obtain an epitaxial TiN film on Si (100) substrate. In the second part, further growth of diamond on the fabricated TiN/Si(100)by microwave plasma chemical vapor deposition (MPCVD) with bias-enhanced nucleation pretreatment was studied for understanding the microstructural characteristics of diamond film.
In the TiN film growth process, a gas mixture of nitrogen and hydrogen was used for plasma nitriding of 50 nm thick TiO2 which was grown on Si(100) by atomic layer deposition. The orientations and film crystallinities of TiN thin films were found to vary with the plasma nitriding conditions including hydrogen concentration, microwave power, process pressure, and nitridation time. The morphology, crystallinity and chemical boding of TiN after plasma nitriding of TiO2 were characterized by using scanning electron microscopy (SEM), X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), and transmission electron microscopy (TEM). The results show that increasing the hydrogen concentration from 0.4 to 4 % into nitrogen gas can effectively form TiN, and epitaxial TiN of good film quality can be formed with the plasma condition at pressure of 50 torr and power of 700 W.
In the diamond growth process by MPCVD, bias voltage and growth time were varied for diamond nucleation and growth. It is shown that nanocrystalline diamonds with amorphous carbon were formed on top of TiN with a nucleation density ~ 1.5 x 109 cm-2 after biasing. Further growth can result in formation of an oriented diamond film.
In the TiN film growth process, a gas mixture of nitrogen and hydrogen was used for plasma nitriding of 50 nm thick TiO2 which was grown on Si(100) by atomic layer deposition. The orientations and film crystallinities of TiN thin films were found to vary with the plasma nitriding conditions including hydrogen concentration, microwave power, process pressure, and nitridation time. The morphology, crystallinity and chemical boding of TiN after plasma nitriding of TiO2 were characterized by using scanning electron microscopy (SEM), X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), and transmission electron microscopy (TEM). The results show that increasing the hydrogen concentration from 0.4 to 4 % into nitrogen gas can effectively form TiN, and epitaxial TiN of good film quality can be formed with the plasma condition at pressure of 50 torr and power of 700 W.
In the diamond growth process by MPCVD, bias voltage and growth time were varied for diamond nucleation and growth. It is shown that nanocrystalline diamonds with amorphous carbon were formed on top of TiN with a nucleation density ~ 1.5 x 109 cm-2 after biasing. Further growth can result in formation of an oriented diamond film.