氧化鋁鋅/氧化矽/矽異質接面結構之光檢測器研究

A Study of Photodetectors Based on AZO/SiOx/n-Si Heterojunction Structure

檔案

全文未公開。

日期

2015

類型

語言

中文

摘要

本研究探討由氧化鋁鋅(Alumium-doped Zinc Oxide,AZO)/氧化矽(Silicon Oxide,SiOx)/n型矽(n-Silicon,n-Si)組成之半導體/絕緣層/半導體異質接面(Semiconductor-Insulator-Semiconductor Heterojunction Structure,SISHJS)結構於光檢測器之應用。先以乾式熱氧化法(Dry Thermal Oxidation)在n-Si基板上成長數奈米厚之SiOx層作為SIS元件之絕緣層,再以濺鍍法(Sputtering)將AZO薄膜沉積於SiOx上,最後以電子束蒸鍍法(e-beam Evaporation)蒸鍍鋁(Alumium,Al)為上下電極完成SIS元件之製備。首先探討在不加熱基板的條件下沉積之AZO薄膜性質,所有AZO薄膜皆有大於80%之平均光穿透率,並發現隨著薄膜厚度增加,平均光穿透率隨之降低,而電阻率(Resistivity)則隨厚度增加降低,以250 W之濺鍍功率沉積、且厚度為400 nm的AZO薄膜具有最低之電阻率值9.20×10-4 Ω-cm。
本研究共探討AZO薄膜濺鍍功率、薄膜厚度、後退火處理及SiOx層厚度對於SIS元件光檢測性質之影響。隨著AZO薄膜濺鍍功率的增加,SIS元件之光響應度(Photoresponse,R)愈佳;SIS元件之AZO薄膜以200 nm為最佳厚度,大於200 nm將降低光穿透率而減少光激發載子數目而降低R值,低於200 nm時AZO之電阻率值升高而提高元件串聯電阻,因而降低R值;SIS元件試片經300oC、大氣氣氛退火1 hr可顯著提升R值,退火可使元件之界面缺陷密度(Interface Trap Density,Dit)由1.63×1012 eV-1cm-2降至2.80×1011 eV-1cm-2,此降低光激發載子被界面缺陷捕捉之機率而提升R值,退火溫度高於300oC則會大幅提高AZO之電阻率值,此增加元件串聯電阻而降低R值;SiOx層厚度約為2.0 nm時可得到最佳R值,厚度小於2.0 nm者無法有效分離光激發之電子-電洞對;大於2.0 nm者則會降低載子穿隧機率使穿隧電流下降,此使SIS元件之串聯電阻增大而降低R值。歸納上述研究可得到厚度為2.0 nm之SiOx層、以250 W濺鍍功率鍍著200 nm厚之AZO薄膜並經300oC、大氣氣氛退火1 hr之SIS元件具有最佳之光檢測性質,在365、650及940 nm波段入射光照射下之R值分別為0.27、1.60及0.67 AW-1,並具有小於10 msec之快速響應時間。
This study investigates the feasibility of aluminum-doped zinc oxide/silicon oxide/n-type silicon (AZO/SiOx/n-Si) semiconductor/insulator/semiconductor heterojunction structure (SISHJS) to photodetection. The SIS structure was prepared firstly by growing an ultra-thin SiOx layer on n-type Si wafer substrate via the dry thermal oxidation. Radio-frequency sputtering was then adopted to deposit the AZO layer on SiOx/n-Si substrate. Afterward, the 100-nm-thick aluminum (Al) layers were deposited by e-beam evaporation to form the bottom electrodes on the backside of Si substrates and the top finger electrodes on AZO layer, respectively, to complete the preparation of SIS photodetector samples.
The AZO layers were deposited by sputtering process without substrate heating and all of them exhibited the average transmittance greater than 80 % in visible-light wavelength range. The lowest resistivity of 9.20×10-4 Ω-cm was achieved in 400-nm thick AZO layer deposited at the sputtering power of 250 W. Afterward, the influence of sputtering power and thicknesses of AZO layers, post-annealing conditions and SiOx layer thicknesses on the SIS device performance was investigated. Analytical results indicated that the photoresponse (R) of SIS devices improves as the sputtering power of AZO layer increases. The optimum AZO thicknesses for SIS device was found to be 200 nm that thick AZO inhibits light transmittance and consequently reduces the number of photo-induced carriers whereas the resistivity value of thin AZO would be high to escalates the series resistance of SIS devices. The SiOx insulating layer with thickness of 2 nm was appropriate for SIS devices that thin SiOx layer cannot effectively separate the photo-induced electron-hole pairs whereas thick SiOx layer retards the tunneling of carriers and increases the series resistance of SIS devices. Post annealing at 300oC for 1 hr could improve the R values significantly since it reduced the interface trap densities (Dit) at the AZO/SiOx and SiOx/n-Si interfaces from 1.63×1012 eV-1cm-2 to 2.80×1011 eV-1cm-2 and effectively suppressed the carrier capture at the interfaces.
The optimum R values were 0.27, 1.60 and 0.67 AW-1 separately under the 365-nm, 650-nm and 940-nm illuminations and with the fast response time less than 10 msec observed in SIS device containing 2.0-nm thick SiOx layer, 200-nm thick AZO layer deposited at sputtering power of 250 W and subjected to the 300oC-annealing in air ambient for 1 hr.
顯示完整詮釋資料 統計資料

引用此條目

吳秉謙 (2015). 氧化鋁鋅/氧化矽/矽異質接面結構之光檢測器研究. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/62399