提升大面積綠色磷光有機發光二極體元件壽命
Improving the lifetime of large-area green phosphorescent organic light-emitting diodes by solution process
摘要
本論文主要是以液態刮刀製程進行大面積綠色磷光有機發光二極體之壽命研究。藉由改變元件結構、改善成膜性、調變膜厚、改善封裝,藉此提升大面積綠色磷光的電性及壽命表現。現今有機發光二極體製程方面尚以蒸鍍製程為主流,蒸鍍製程相對穩定且良率佳,但其不易進行大面積元件製作以及設備昂貴、製程時間長等缺點。本論文所使用之製程為液態刮刀塗佈製程,其優勢在高度材料利用性、低製程時間、設備相對簡易與易於進行大面積塗佈等,本論文將以此技術進行大面積元件製作與探討。
由於多層結構對液態製程及大面積塗佈來說有一定的困難性,故本論文基本上以單層結構元件為主要研究項目,其結構為ITO/PEDOT:PSS/SPPO13:TCTA:Ir/LiF/Al,結果顯示在電洞注入層(PEDOT:PSS)與發光層(SPPO13:TCTA:Ir)間加入一層很薄之電洞傳輸層材料並搭配CsF/Al電極可將電流效率從10 cd/A提升至20 d/A,且若再將界面活性劑加入至電洞注入層中,透過改善電洞注入層的成膜性,電流效率最高可達到33 cd/A,而操作壽命方面從一開始元件點亮即瞬間燒毀至最後在500 nits下開始量測T50壽命可達10小時以上。
由於多層結構對液態製程及大面積塗佈來說有一定的困難性,故本論文基本上以單層結構元件為主要研究項目,其結構為ITO/PEDOT:PSS/SPPO13:TCTA:Ir/LiF/Al,結果顯示在電洞注入層(PEDOT:PSS)與發光層(SPPO13:TCTA:Ir)間加入一層很薄之電洞傳輸層材料並搭配CsF/Al電極可將電流效率從10 cd/A提升至20 d/A,且若再將界面活性劑加入至電洞注入層中,透過改善電洞注入層的成膜性,電流效率最高可達到33 cd/A,而操作壽命方面從一開始元件點亮即瞬間燒毀至最後在500 nits下開始量測T50壽命可達10小時以上。
The main purpose of this thesis is to improve the lifetime in large-area green phosphorescent organic light-emitting diodes by solution process. By changing the device structure, modulating parameters and improving package equipment, the lifetime and electrical performance of our devices were improved. Blade coating process is a sort of solution process which can coat nanoscale thin film uniformly. It has several advantages in comparison with the mainstream vacuum manufacturing process, such as fewer quantities of material consumption, lower cost on equipment, much less production time and easier to coat large-area thin film. Because of these advantages, we use this technology to manufacture large-area OLEDs and discuss their electrical performance.
Because the solution process still has some difficulties to manufacture a multilayer structure OLED, our research is basically on single-layer structure OLEDs. Based on our experimental results, the structure of single-layer OLEDs—ITO/PEDOT:PSS/SPO13:TCTA:Ir/ LiF/Al—has average current efficiency of 10 cd/A. If we added a thin layer of cross-linked hole transporting material (TFB) between HIL and EML, with CsF/Al electrode, the average current efficiency would increase from 10 to 20 cd/A. Finally, we improved the flatness of the hole injection layer which is doped with surfactant. The highest current efficiency increased to 33 cd/A and the operated lifetime can achieve up to 10 hours under the initial luminance of 500 cd/m2.
Because the solution process still has some difficulties to manufacture a multilayer structure OLED, our research is basically on single-layer structure OLEDs. Based on our experimental results, the structure of single-layer OLEDs—ITO/PEDOT:PSS/SPO13:TCTA:Ir/ LiF/Al—has average current efficiency of 10 cd/A. If we added a thin layer of cross-linked hole transporting material (TFB) between HIL and EML, with CsF/Al electrode, the average current efficiency would increase from 10 to 20 cd/A. Finally, we improved the flatness of the hole injection layer which is doped with surfactant. The highest current efficiency increased to 33 cd/A and the operated lifetime can achieve up to 10 hours under the initial luminance of 500 cd/m2.