中溫型單片燃料電池LCVO/LSGM/LSCF的組裝與電化學性質測量

Fabrication, Characterization and Electrochemical Measurements of LCVO/LSGM/LSCF Single Cell as Intermediate Temperature Solid Oxide Fuel Cell

檔案

全文未公開。

日期

2018

類型

語言

英文

摘要

本篇論文以甘胺酸燃燒法(glycine-nitrate method)合成實驗室開發之釩離子部分取代Ce位置之La2Ce2O7化合物,並結合商用陰極材料(La0.60Sr0.40)0.95Co0.20Fe0.80O3-δ (LSCF)與電解質材料La0.8Sr0.2Ga0.8Mg0.2O3-(LSGM),在新測試裝置環境下測試電化學性質。同時,對於陶瓷片的製程進行一系列研究,來製備燃料電池片。
在陶瓷片製程中,我們利用刮刀塗布法製備電解質支撐電池,找到適當的行星式球磨機混合流程及最佳溶劑比例來塗布平整、無氣泡之生胚,再利用熱重分析儀找出此生胚在178.2°C到197.4°C和358.8°C到394.7°C兩個區間有明顯的吸熱反應,來改善最佳燒結流程。而最後平整化流程,以每小時兩百攝氏溫度升溫速率提升製目標溫度壓燒陶瓷片進而壓平陶瓷片來製作電池。
在單電池測量裝置中,利用實驗室自製玻璃膠應用於電池封裝取代以往使用的陶瓷膠,並研究其在800°C下可以忍受流速0.09L/min之氮氣。在半電池La2(Ce0.8V0.2)2O7--LSGM/LSGM實驗中發現主要開路電壓由陽極貢獻,而LSGM/LSCF-LSGM陰極半電池在600°C到750°C 的LSGM離子導電度比純電解質片LSGM之離子導電度高,而在800°C,純電解質片之離子導電大於陰極半電池。
比較LCVO-LSGM/LSGM/LSCF-LSGM和LCVO/LSGM/LSCF,陰陽極混入電解質之效果,兩者電池OCP在600°C到800°C之間皆介於1.08 V至1.14 V之間,表示其封裝狀態良好,然而前者之功率密度遠低於後者,經重複實驗與SEM發現,前者之LCVO實質含量偏低,且LSGM混入陽極之後其孔隙比後者少,因此LCVO/LSGM/LSCF單電池功率密度高達0.389 W/cm2。
In this thesis, La2(Ce2V0.2)2O7-δ (LCVO),developed by our lab, was synthesized by glycine-nitrate method. LCVO combines with commercial electrolyte material La0.8Sr0.2Ga0.8Mg0.2O3-(LSGM) and commercial cathode material (La0.60Sr0.40)0.95Co0.20Fe0.80O3-δ to study the performance of single cell at new device. At the same time, we study the fabrication of ceramics to improve the quality of single cells.
For the fabrication, we used Tape casting method to fabricate electrolyte-supported cells. And we found out the best ratio of solvents and milling program of slurry which was milled by Planetary Mills, and we can produce green tape without the bubbles. TGA told us there were endothermic reaction at two ranges: from 178.2°C to 197.4°C and from 358.8°C to 394.7°C. We modified the sintering program based on this result. Last step, we pressed the ceramic by the alumina plates and sintered at target temperature with 200°C /h to flatter the ceramics.
We used Pyrex glass sealant, made by our lab, to replace the previous ceramics sealant, and found this glass sealant can tolerate up to 0.09L/min flow rate at 800°C. For anode half cell, we found that the major open circuit potential (OCP) was provided by anode cite. For cathode half cell, ionic conductivity of LSGM was higher than pure LSGM from 600°C to 750°C. Instead, ionic conductivity of pure LSGM was higher than LSGM of cathode half cell at 800°C.
For LCVO-LSGM/LSGM/LSCF-LSGM and LCVO/LSGM/LSCF, OCP of both cells were bewtween 1.08 V and 1.14 V, and the cells were considered to be sealed well between 600°C and 800°C. However, the former’s power density is lower than the latter one. Repeating experiments and based on SEM, the LCVO content of the former is less than the latter. LSGM, mixed with LCVO, made the porosity of anode less than pure LCVO anode. Therefore, the power density of LCVO/LSGM/LSCF could reach to 0.389 W/cm2。
顯示完整詮釋資料 統計資料

引用此條目

Lin, Y.-C. (2018). Fabrication, Characterization and Electrochemical Measurements of LCVO/LSGM/LSCF Single Cell as Intermediate Temperature Solid Oxide Fuel Cell. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/67950

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/67950