本論文透過改變下方單晶矽基板為複晶矽層,成功地增加矽間隙子於氧化過程中釋放的量。並有效地調控一體成型之鍺量子點/二氧化矽/矽鍺殼層的異質結構參數,使原先唇型的矽鍺殼層轉變為整層複晶矽鍺層。透過能量散佈分析儀(Energy Dispersive X-ray, EDX)觀察到鍺會隨著複晶矽之晶界而分布在其中,顯示矽間隙子釋放的均勻度亦為重要考量參數之一。
透過掏空鍺量子點周圍之氮化矽的方式,可使60 nm和90 nm鍺量子點分別減少2.12%(2.15 GPa)和0.47%(0.44 GPa)的壓縮應力。此結果顯示掏空氮化矽有助於鍺量子點釋放其壓縮應力,更進一步實驗驗證了鍺量子點的壓縮應力是源自於氮化矽薄膜擠壓的推論。由低溫光激發螢光光譜可得知,60 nm和90 nm鍺量子點的訊號峰值能量分別為0.801 eV和0.803 eV。根據訊號峰值能量對激發功率和溫度的相依性,可知鍺量子點的放光機制是屬於載子在直接能隙處的輻射性複合。以上結果顯示一體成型鍺量子點具有做為高發光效益矽基光源的潛力。
量測以鍺量子點做為本質層之P-I-N光偵測元件。當元件偏壓為-0.7 V,入射光功率調整在2.2到3.4 mW,量測溫度在77 K時,其在850 nm、1310 nm和1550 nm波段下的光增益分別為593、295和47 A/A。顯示鍺量子點在近紅外光波段具有明顯的光偵測特性。
透過掏空鍺量子點周圍之氮化矽的方式,可使60 nm和90 nm鍺量子點分別減少2.12%(2.15 GPa)和0.47%(0.44 GPa)的壓縮應力。此結果顯示掏空氮化矽有助於鍺量子點釋放其壓縮應力,更進一步實驗驗證了鍺量子點的壓縮應力是源自於氮化矽薄膜擠壓的推論。由低溫光激發螢光光譜可得知,60 nm和90 nm鍺量子點的訊號峰值能量分別為0.801 eV和0.803 eV。根據訊號峰值能量對激發功率和溫度的相依性,可知鍺量子點的放光機制是屬於載子在直接能隙處的輻射性複合。以上結果顯示一體成型鍺量子點具有做為高發光效益矽基光源的潛力。
量測以鍺量子點做為本質層之P-I-N光偵測元件。當元件偏壓為-0.7 V,入射光功率調整在2.2到3.4 mW,量測溫度在77 K時,其在850 nm、1310 nm和1550 nm波段下的光增益分別為593、295和47 A/A。顯示鍺量子點在近紅外光波段具有明顯的光偵測特性。
In this thesis, We successfully increased the amount of Si interstitials released during thermal oxidation process by replacing c-Si substrate with poly-Si layer. The cup-shaped SiGe shell in the self-organized Ge-QD/SiO2/SiGe shell heterostructure was also observed to become a poly-SiGe layer. Indicating that we can effectively tune the structure parameter of the heterostructure by changing the crystallinity of Si substrate. From the EDX mapping results, we found that Ge distribution within the poly-Si layer was non-uniform and segregated along the grain-boundary. These results show that not only the amount but also the uniformity of Si interstitials released are the important factors for heterostructure tuning.
By etching the Si3N4 beside the Ge-QD, a reduction in 2.12%(2.15 GPa) and 0.47%(0.44 GPa) compressive strain of the 60 nm and 90 nm Ge-QD was observed, respectively. This result experimentally proved the inference that the compressive strain of Ge-QD was from the Si3N4 layer during the QD formation. According to the photoluminescence spectra, the peak value of the 60 nm and 90 nm Ge-QD was 0.801 eV and 0.803 eV, respectively. The power and temperature dependence of the PL spectra indicated the direct bandgap transition and radiative recombination of the exitons in the Ge-QD. This shows the potential of the self-organized Ge-QD in achieving high efficiency light source for Si-based optical interconnect.
The photocurrent gain was measured on Ge-QD P-I-N photodetector at 77 K. At the voltage of -0.7 V, the photocurrent gain were 593, 295 and 47 A/A for 850 nm, 1310 nm and 1550 nm laser, respectively, under the incident power controlled from 2.2 mW to 3.4 mW. Indicating the Ge-QD has significant photodetection characteristics in the near-infrared regime.
By etching the Si3N4 beside the Ge-QD, a reduction in 2.12%(2.15 GPa) and 0.47%(0.44 GPa) compressive strain of the 60 nm and 90 nm Ge-QD was observed, respectively. This result experimentally proved the inference that the compressive strain of Ge-QD was from the Si3N4 layer during the QD formation. According to the photoluminescence spectra, the peak value of the 60 nm and 90 nm Ge-QD was 0.801 eV and 0.803 eV, respectively. The power and temperature dependence of the PL spectra indicated the direct bandgap transition and radiative recombination of the exitons in the Ge-QD. This shows the potential of the self-organized Ge-QD in achieving high efficiency light source for Si-based optical interconnect.
The photocurrent gain was measured on Ge-QD P-I-N photodetector at 77 K. At the voltage of -0.7 V, the photocurrent gain were 593, 295 and 47 A/A for 850 nm, 1310 nm and 1550 nm laser, respectively, under the incident power controlled from 2.2 mW to 3.4 mW. Indicating the Ge-QD has significant photodetection characteristics in the near-infrared regime.