牙科贋復治療用短玻璃纖維根柱開發與生物力學探討
Development and biomechanics of short glass fiber post system for dental prosthetic treatment
摘要
贋復治療過程中置入根柱,可增加牙齒抵抗斷裂的強度,已成為牙科進行贋復治療必要的修復步驟。近年來發展出了玻璃纖維的根柱,其優點為使用方便、色澤透明且彎曲係數比較接近牙本質。然而,目前市售產品因受限於材料與加工製程關係,無法完全符合臨床之適配性(adaptation)、強度(strength)、阻光(Radiopacity)、導光(light transmission)、黏著(bounding)與移除(removal)等需求,在臨床使用上仍有改進空間。
本研究以短纖玻璃纖維為基材並利用微小射出成型製程,製造與小臼齒根管外型適配性較佳之解剖短纖維根柱(SGFR-Post)。探討市售實心長纖維(X-Post)、中空長纖維(Q-Post)與自行開發解剖短纖維根柱(SGFR-Post)進行實驗。實驗可分為體外力學實驗與臨床需求實驗兩大部分。體外力學實驗包含根柱本體彎曲強度與自然牙齒生物力學實驗,包含軸向45度靜態與疲勞負載實驗,並全程配合音洩訊號偵測。將實驗後之樣品,以CEJ、CEJ下1.5mm與1/2牙齒長度橫向切割,觀察內部破壞情況。臨床需求實驗包含根柱三點彎曲、阻光(顯影)、導光、推出(黏著強度)、根柱移除五項實驗,來探討彼此間的影響關係與臨床重要性。
本研究實驗結果發現,市售長纖X-Post彎曲強度與模數為925.8±55.9MPa/25.8±0.48GPa,短纖SGFR-Post為743.2±11.4MPa/28.1±1.94GPa。自然牙齒力學實驗結果,在靜態實驗結果SGFR-Post為690.3±53.36N,X-Post為617.6±51.79N。疲勞負載實驗SGFR-Post最終以207.1N通過120萬次疲勞負載,X-Post為185.3N 通過。音洩累積訊號次數SGFR-Post為153.0次,X-Post為194.7次。觀察內部破壞情況,SGFR-Post明顯的破壞裂紋平均為2.44±1.42個,X-Post為4.78±2.68個。在臨床需求實驗結果,阻光實驗結果,三款纖維根柱均能透過X光拍攝清楚分辨根柱在牙齒內部之位置。導光實驗結果發現短纖SGFR-Post與中空長纖Q-Post在超過8mm後均無能量(光)傳遞,而X-Post在16mm仍可偵測到能量(光)。黏著強度方面,在兩種黏合劑組別下SGFR-Post、Q-Post與X-Post均有隨牙髓腔深度力量遞減的趨勢,自行固化(Self-cure)組別三種根柱同一層力量無顯著差異。雙向固化(Dual-cure)的黏合劑實驗結果發現在第三層(12mm) ,推出力量為SGFR-Post(4.45N/mm2)、Q-Post(4.19N/mm2)與X-Post(6.18N/mm2)。根柱移除實驗結果,不具臨床經驗者移除時間/黏合劑殘餘體積分別為SGFR-Post(1685±89秒/16.8±1.2%)、Q-Post(1433±58秒/15.4±2.0%)與X-Post(1626±73秒/13.2±1.6%),具臨床經驗者為SGFR-Post(1267±71秒/9.3±1.0%)、Q-Post(727±38秒/8.2±0.6%)與X-Post(1039±113秒/8.4±0.8%)。
本研究已成功開發出解剖短纖維根柱(SGFR-Post),雖然在彎曲強度較市售長纖產品低,但在置入牙齒後之力學表現優於市售產品。臨床需求實驗短纖根柱可從X光影像中觀察在牙齒之位置。導光特性卻不如長纖實心根柱。黏著強度在Self-cure黏合
劑表現無太大差異,但在Dual-cure表現卻因光傳遞不足而降低黏著強度。中空根柱對於臨床經驗者,移除時間最少且成效最好。本研究開發之解剖短纖維根柱在力學實驗中表現有其優勢,然而臨床需求實驗仍有不足的地方。因此,本研究解剖短纖維根柱設計與開發,可提供臨床贋復治療時纖維根柱更多的選擇與參考,臨床需求實驗設計可提供牙科根柱開發相關學術實驗方法與研究之參考價值。
本研究以短纖玻璃纖維為基材並利用微小射出成型製程,製造與小臼齒根管外型適配性較佳之解剖短纖維根柱(SGFR-Post)。探討市售實心長纖維(X-Post)、中空長纖維(Q-Post)與自行開發解剖短纖維根柱(SGFR-Post)進行實驗。實驗可分為體外力學實驗與臨床需求實驗兩大部分。體外力學實驗包含根柱本體彎曲強度與自然牙齒生物力學實驗,包含軸向45度靜態與疲勞負載實驗,並全程配合音洩訊號偵測。將實驗後之樣品,以CEJ、CEJ下1.5mm與1/2牙齒長度橫向切割,觀察內部破壞情況。臨床需求實驗包含根柱三點彎曲、阻光(顯影)、導光、推出(黏著強度)、根柱移除五項實驗,來探討彼此間的影響關係與臨床重要性。
本研究實驗結果發現,市售長纖X-Post彎曲強度與模數為925.8±55.9MPa/25.8±0.48GPa,短纖SGFR-Post為743.2±11.4MPa/28.1±1.94GPa。自然牙齒力學實驗結果,在靜態實驗結果SGFR-Post為690.3±53.36N,X-Post為617.6±51.79N。疲勞負載實驗SGFR-Post最終以207.1N通過120萬次疲勞負載,X-Post為185.3N 通過。音洩累積訊號次數SGFR-Post為153.0次,X-Post為194.7次。觀察內部破壞情況,SGFR-Post明顯的破壞裂紋平均為2.44±1.42個,X-Post為4.78±2.68個。在臨床需求實驗結果,阻光實驗結果,三款纖維根柱均能透過X光拍攝清楚分辨根柱在牙齒內部之位置。導光實驗結果發現短纖SGFR-Post與中空長纖Q-Post在超過8mm後均無能量(光)傳遞,而X-Post在16mm仍可偵測到能量(光)。黏著強度方面,在兩種黏合劑組別下SGFR-Post、Q-Post與X-Post均有隨牙髓腔深度力量遞減的趨勢,自行固化(Self-cure)組別三種根柱同一層力量無顯著差異。雙向固化(Dual-cure)的黏合劑實驗結果發現在第三層(12mm) ,推出力量為SGFR-Post(4.45N/mm2)、Q-Post(4.19N/mm2)與X-Post(6.18N/mm2)。根柱移除實驗結果,不具臨床經驗者移除時間/黏合劑殘餘體積分別為SGFR-Post(1685±89秒/16.8±1.2%)、Q-Post(1433±58秒/15.4±2.0%)與X-Post(1626±73秒/13.2±1.6%),具臨床經驗者為SGFR-Post(1267±71秒/9.3±1.0%)、Q-Post(727±38秒/8.2±0.6%)與X-Post(1039±113秒/8.4±0.8%)。
本研究已成功開發出解剖短纖維根柱(SGFR-Post),雖然在彎曲強度較市售長纖產品低,但在置入牙齒後之力學表現優於市售產品。臨床需求實驗短纖根柱可從X光影像中觀察在牙齒之位置。導光特性卻不如長纖實心根柱。黏著強度在Self-cure黏合
劑表現無太大差異,但在Dual-cure表現卻因光傳遞不足而降低黏著強度。中空根柱對於臨床經驗者,移除時間最少且成效最好。本研究開發之解剖短纖維根柱在力學實驗中表現有其優勢,然而臨床需求實驗仍有不足的地方。因此,本研究解剖短纖維根柱設計與開發,可提供臨床贋復治療時纖維根柱更多的選擇與參考,臨床需求實驗設計可提供牙科根柱開發相關學術實驗方法與研究之參考價值。
To place the post in to the root during endodontical treatment has become an important procedure for dental restoration. As the aesthetic trend, the glass fiber posts were developed to have more favorable young’s modulus as dentin and translucent feature in current. Therefore, the glass fiber posts are getting popular in clinical use, even more reason for dental restoration with ceramic crown, especially in frontal tooth. However, the current fiber post are not fully compatible with adaptation, strength, radiopacity, light transmission, bounding and removal properties in clinical use and post profiles are constrained by inherent manufacturing process and material issues.
The purpose of this project is developing the manufacturing process of injection molding using short glass fiber to design a novel anatomical short glass fiber reinforced post(SGFR-Post) with clinical expected. Five experiments were performed for fiber post mechanical test of in this study included 3-point bending, torsion resistance, push out, light transmission and removal test to explore the performance of the SGFR-Post, long-fiber(X-Post) and hallow(Q-Post) posts. In vitro mechanical experiments including the static and fatigue test that was designed to drive a 45° oblique load onto the functional cusp of each restored tooth, and during the static and fatigue tests an AE signal wide band transducer was glued with resin to the resin block in which the sample was embedded. After testing the samples were cut with CEJ, CEJ under 1.5mm and 1/2 tooth length, and the internal damage was observed.
The results showed that the flexural strength/modulus of SGFR-Post (743.2±11.4MPa/28.1±1.94GPa) was significantly lower than X-Post (925.8±55.9MPa/25.8±0.48GPa) (P <0.05). The static fracture resistance results were 690.3±53.36 N and 617.6±51.79 N for an endodontically treated tooth used with SGFR and commercial FRC posts, respectively. SGFR post presented higher resistance than the commercial FRC post (p<0.05). A load-cycle result showed that the endurance limitation at 1.2×106 cycles was 207.1 N for the anatomical SGFR fiber post. This value was higher than 185.3 N found in the commercial FRC post. The number of AE signals increased with the cycle load number and the accumulated average number of AE signals for the anatomical SGFR fiber post (153.0) was significantly lower than that for the commercial FRC post (194.7) under 40% of the static maximum resistance fatigue test load (p<0.05). The result showed that the average number of micro cracks for the restored tooth using the commercial FRC post (4.78) was significantly higher than those in the tooth using the anatomical SGFR (2.44) (p<0.05). All fiber post can be clearly to distinguish the dentin, cement and post position in internal of teeth by X-ray image. The light transmission showed that SGFR-Post and Q-Post had no energy (light) more than 8mm depth, but SGF post can detect energy (light) over 16mm depth. The push out strength of all posts were decreased with the depth of the pulp cavity in the two adhesive groups. Self-cure group had no significant difference of the same layer. The push out strength of dual-cure cement group was SGFR-Post (4.45N / mm2), Q-Post (4.19N / mm2) and X-Post (6.18N / mm2) in the third layer (12mm). The results of post removal experiment showed that Q-Post (1433 ± 58 sec / 15.4 ± 2.0%) and X-Post with no clinical experience and Q-Post (727 ± 38 seconds / 8.2 ± 0.6%) and X-Post (1039 ± 113 seconds / 8.4 ± 0.8%) with clinical experience.
This study demonstrated that the novel anatomical SGFR fiber post with enhanced retention designs made using precise injection molding presented superior static fracture resistance and fatigue endurance limitations than the commercial FRC post. The accumulated number of micro cracks for a restored tooth using the commercial FRC post was significantly higher than that using the anatomical SGFR fiber post in fatigue testing. The SGFR-Post through the X-ray image is clearly visible inside the teeth, but light transmission ability was lower than long fiber post. The bonding strength in self-cure adhesives showed no significant difference in the same layer, but in the dual-cure the strength decrease with depth. Hollow structure post for clinical experience can save time and more complete removal. The SGFR-Post developed in this study has its advantages in mechanical experiments, but there are still some limitations in clinical trials. Therefore, this study of SGFR-Post design and development can provide endodontic retreatment and dental fiber post another choice, the experimental design could provide dental related research reference.
The purpose of this project is developing the manufacturing process of injection molding using short glass fiber to design a novel anatomical short glass fiber reinforced post(SGFR-Post) with clinical expected. Five experiments were performed for fiber post mechanical test of in this study included 3-point bending, torsion resistance, push out, light transmission and removal test to explore the performance of the SGFR-Post, long-fiber(X-Post) and hallow(Q-Post) posts. In vitro mechanical experiments including the static and fatigue test that was designed to drive a 45° oblique load onto the functional cusp of each restored tooth, and during the static and fatigue tests an AE signal wide band transducer was glued with resin to the resin block in which the sample was embedded. After testing the samples were cut with CEJ, CEJ under 1.5mm and 1/2 tooth length, and the internal damage was observed.
The results showed that the flexural strength/modulus of SGFR-Post (743.2±11.4MPa/28.1±1.94GPa) was significantly lower than X-Post (925.8±55.9MPa/25.8±0.48GPa) (P <0.05). The static fracture resistance results were 690.3±53.36 N and 617.6±51.79 N for an endodontically treated tooth used with SGFR and commercial FRC posts, respectively. SGFR post presented higher resistance than the commercial FRC post (p<0.05). A load-cycle result showed that the endurance limitation at 1.2×106 cycles was 207.1 N for the anatomical SGFR fiber post. This value was higher than 185.3 N found in the commercial FRC post. The number of AE signals increased with the cycle load number and the accumulated average number of AE signals for the anatomical SGFR fiber post (153.0) was significantly lower than that for the commercial FRC post (194.7) under 40% of the static maximum resistance fatigue test load (p<0.05). The result showed that the average number of micro cracks for the restored tooth using the commercial FRC post (4.78) was significantly higher than those in the tooth using the anatomical SGFR (2.44) (p<0.05). All fiber post can be clearly to distinguish the dentin, cement and post position in internal of teeth by X-ray image. The light transmission showed that SGFR-Post and Q-Post had no energy (light) more than 8mm depth, but SGF post can detect energy (light) over 16mm depth. The push out strength of all posts were decreased with the depth of the pulp cavity in the two adhesive groups. Self-cure group had no significant difference of the same layer. The push out strength of dual-cure cement group was SGFR-Post (4.45N / mm2), Q-Post (4.19N / mm2) and X-Post (6.18N / mm2) in the third layer (12mm). The results of post removal experiment showed that Q-Post (1433 ± 58 sec / 15.4 ± 2.0%) and X-Post with no clinical experience and Q-Post (727 ± 38 seconds / 8.2 ± 0.6%) and X-Post (1039 ± 113 seconds / 8.4 ± 0.8%) with clinical experience.
This study demonstrated that the novel anatomical SGFR fiber post with enhanced retention designs made using precise injection molding presented superior static fracture resistance and fatigue endurance limitations than the commercial FRC post. The accumulated number of micro cracks for a restored tooth using the commercial FRC post was significantly higher than that using the anatomical SGFR fiber post in fatigue testing. The SGFR-Post through the X-ray image is clearly visible inside the teeth, but light transmission ability was lower than long fiber post. The bonding strength in self-cure adhesives showed no significant difference in the same layer, but in the dual-cure the strength decrease with depth. Hollow structure post for clinical experience can save time and more complete removal. The SGFR-Post developed in this study has its advantages in mechanical experiments, but there are still some limitations in clinical trials. Therefore, this study of SGFR-Post design and development can provide endodontic retreatment and dental fiber post another choice, the experimental design could provide dental related research reference.