非晶氧化銦鎢奈米薄片電晶體源極/汲極工程之研究
Study on Source/Drain Engineering of Amorphous Indium Tungsten Oxide Nano-Sheet Transistors
摘要
近年來,非晶態金屬氧化物半導體(Amorphous Oxide Semiconductor, AOS)發展迅速,因其具有高的載子遷移率(mobility)、低製程溫度、高透明性、以及相容於現有顯示器製程且成本低廉的優勢。在眾多的非晶態金屬氧化物半導體中,又以具良好特性之非晶態氧化銦鎵鋅(a-IGZO)材料被最為廣泛研究。然而,隨著顯示技術的日新月異,對於未來大尺寸面板、超高畫質顯示、有機發光二極體驅動、軟性電子等應用上,銦鎵鋅氧化物半導體已漸漸不敷需求。為此,本論文開發高效能、低功耗的非晶態氧化銦鎢奈米薄片電晶體(a-InWO Nano-Sheet Transistors, a-IWO NSTs),此新穎元件的優勢為:(1) 利用高載子遷移率的氧化銦作為通道薄片主體,並摻入少量的鎢元素取代較昂貴的鎵元素,藉由較高之鎢及氧的解離能(bond-dissociation energy)以抑制多餘的氧空缺,進而提高元件穩定性; (2) 利用超薄之氧化銦鎢奈米薄片(約為3.5奈米)作為通道,並且利用高介電係數之二氧化鉿(HfO2)作為元件之閘極絕緣層製成具有低臨界電壓(threshold voltage)、優異的次臨界擺幅(subthreshold swing)以及高的驅動電流(drain current)和開關電流比(Ion/Ioff)等優秀特性之電晶體元件。藉由此無接面(junctionless)的氧化銦鎢奈米薄片電晶體,在元件關閉時能達到通道全空乏(fully depletion)以降低漏電流及提升閘極對通道之控制能力,增加元件開關切換速率。我們也藉由電容-電壓特性的量測,不僅萃取出閘極絕緣層之介電係數,搭配穿透式電子顯微鏡(Transmission Electron Microscopy, TEM)影像,更可以觀察到元件具有良好之通道/閘極絕緣層沉積剖面。
另外,我們更詳細探討了三種不同功函數材料,鉬(Mo)、氧化銦鎢/鉬堆疊結構(IWO/Mo)和鎳(Ni)作為源極/汲極時對元件的影響。舉凡臨界電壓下降(VTH roll-off),次臨界擺幅的變化以及閘極誘發汲極漏電(Gate Induced Drain Leakage, GIDL)等現象及元件於開啟狀態時的接觸電阻(contact resistance)、場效遷移率等等皆會被詳細探討。我們發現鉬源極/汲極之元件具有最好的開關電流比及場效遷移率源於其具有最小的源極/汲極和通道間的功函數差,進而形成最優良的歐姆接觸和最小的接觸電阻。氧化銦鎢/鉬堆疊結構作為源極/汲極的元件,因為與通道形成同質接面(homojunction)的緣故,則較不受通道長度的影響產生臨界電壓下降之現象。至於鎳源極/汲極之元件,因與通道間有較高的功函數差,在元件開啟時會有較顯著的穿隧電流(tunneling current),從而體現出最優異的次臨界擺幅。最後,我們更研究了元件穩定性議題,藉由新穎之有機負型環氧樹脂(epoxy-based negative photoresist, SU-8)作為通道保護層,並經過一系列的可靠度測試後,如閘極偏壓測試(gate bias stress)、溫度偏壓測試(temperature bias stress)、照光下負偏壓測試(negative bias illumination stress)以及長時間高溫度高濕度的嚴苛環境測試(high temperature/humidity test),發現SU-8材料可大幅提高元件穩定度,驗證其具有相當大之潛力可應用於未來元件之保護層。
在本論文中,我們透過氧化銦鎢奈米薄片作為通道層,搭配高介電係數二氧化鉿作為閘極絕緣層,以及SU-8材料作為通道保護層,成功製造出具不同源極/汲極以及電性特點之奈米薄片電晶體,非常適合用於未來高階顯示、軟性電子、三維晶片(3D IC)及混合互補式金氧半場效應電晶體(hybrid CMOS)等技術。
另外,我們更詳細探討了三種不同功函數材料,鉬(Mo)、氧化銦鎢/鉬堆疊結構(IWO/Mo)和鎳(Ni)作為源極/汲極時對元件的影響。舉凡臨界電壓下降(VTH roll-off),次臨界擺幅的變化以及閘極誘發汲極漏電(Gate Induced Drain Leakage, GIDL)等現象及元件於開啟狀態時的接觸電阻(contact resistance)、場效遷移率等等皆會被詳細探討。我們發現鉬源極/汲極之元件具有最好的開關電流比及場效遷移率源於其具有最小的源極/汲極和通道間的功函數差,進而形成最優良的歐姆接觸和最小的接觸電阻。氧化銦鎢/鉬堆疊結構作為源極/汲極的元件,因為與通道形成同質接面(homojunction)的緣故,則較不受通道長度的影響產生臨界電壓下降之現象。至於鎳源極/汲極之元件,因與通道間有較高的功函數差,在元件開啟時會有較顯著的穿隧電流(tunneling current),從而體現出最優異的次臨界擺幅。最後,我們更研究了元件穩定性議題,藉由新穎之有機負型環氧樹脂(epoxy-based negative photoresist, SU-8)作為通道保護層,並經過一系列的可靠度測試後,如閘極偏壓測試(gate bias stress)、溫度偏壓測試(temperature bias stress)、照光下負偏壓測試(negative bias illumination stress)以及長時間高溫度高濕度的嚴苛環境測試(high temperature/humidity test),發現SU-8材料可大幅提高元件穩定度,驗證其具有相當大之潛力可應用於未來元件之保護層。
在本論文中,我們透過氧化銦鎢奈米薄片作為通道層,搭配高介電係數二氧化鉿作為閘極絕緣層,以及SU-8材料作為通道保護層,成功製造出具不同源極/汲極以及電性特點之奈米薄片電晶體,非常適合用於未來高階顯示、軟性電子、三維晶片(3D IC)及混合互補式金氧半場效應電晶體(hybrid CMOS)等技術。
In recently, Amorphous Oxide semiconductor (AOS) has been developed rapidly due to its advantages on high carrier mobility, high transparency, low cost and compatibility to current display industry. Among various AOS materials, amorphous indium-gallium-zinc oxide (a-IGZO) is the most widely investigated one owing to good electrical performance. It is even considered to be the most potential candidate to serve as channel layer of thin-film transistors in next generation display application. However, technology is ever-changing. Nowadays, a-IGZO cannot satisfy the higher and higher demands gradually from large displays, Ultra-High Definition (UHD), Organic Light Emitted Diodes (OLEDs), flexible electronics and so on. In this study, the transparent amorphous indium-tungsten oxide Nano-Sheet Transistors (a-IWO NSTs) have been developed for achieving high performance and low power consumption. This novel device has several advantages. For instance, we adopted indium oxide based AOS materials with high carrier mobility to serve as channel layer majorly, and doped little tungsten rather than more expensive gallium. We suppressed excess oxygen vacancies in our devices by higher bond-dissociation energy of tungsten-oxygen and enhanced stability of our devices. Moreover, a-IWO with ultra-thin nano-sheet (about 3.5-nm-thick) served as channel layer and high- dielectric, HfO2 served as gate insulator (GI) to achieve excellent performance transistors with low threshold voltage (VTH), outstanding subthreshold swing (S.S.), high on/off current ratio and high driving current. This junctionless a-IWO NST could be fully depleted at off-state to reduce leakage current and improve channel controllability of gate to speed up switching rate. We also measured capacitance-voltage (C-V) characteristics to extract the dielectric constant of GI. Besides, excellent channel/GI profiles from hysteresis-free C-V results and Transmission Electron Microscopy (TEM) images were observed.
Furthermore, we discussed the effects of three different source/drain (S/D) materials with different work functions within a-IWO NSTs in detail. We investigated VTH roll-off, S.S comparison and Gate Induced Drain Leakage (GIDL). For on-state, contact resistance and field-effect mobility (FE) were studied. Devices with Mo S/D had the best on/off current ratio and FE which could be attributed to the smallest work function difference between Mo and a-IWO and formed the perfect ohmic contact by the smallest contact resistance. Devices with IWO/Mo stacking structure S/D had superior performance on VTH roll-off. It is because the homojuction nature at S/D and channel. For Ni S/D device, it showed great S.S due to its significant tunneling phenomenon at subthreshold region originated from the largest work function difference between Ni S/D and a-IWO channel. Finally, we did research about reliability. After passivated our devices by novel epoxy-based negative photoresist, SU-8, and a series stability test such as gate bias stress, temperature bias stress, negative bias illumination stress and rigorous high temperature/humidity test, it showed significant improvement of reliability. Namely, SU-8 has considerable potential in future passivation application.
In this thesis, we adopted a-IWO nano-sheet, high- dielectric,HfO2 and SU-8 to serve as channel, GI and passivation layer respectively to achieve high performance NSTs with different S/D and different electrical advantages. They are definitely suitable for advanced displays, flexible electronics, three-dimensional integrated circuit (3D-IC) and hybrid-CMOS technologies.
Furthermore, we discussed the effects of three different source/drain (S/D) materials with different work functions within a-IWO NSTs in detail. We investigated VTH roll-off, S.S comparison and Gate Induced Drain Leakage (GIDL). For on-state, contact resistance and field-effect mobility (FE) were studied. Devices with Mo S/D had the best on/off current ratio and FE which could be attributed to the smallest work function difference between Mo and a-IWO and formed the perfect ohmic contact by the smallest contact resistance. Devices with IWO/Mo stacking structure S/D had superior performance on VTH roll-off. It is because the homojuction nature at S/D and channel. For Ni S/D device, it showed great S.S due to its significant tunneling phenomenon at subthreshold region originated from the largest work function difference between Ni S/D and a-IWO channel. Finally, we did research about reliability. After passivated our devices by novel epoxy-based negative photoresist, SU-8, and a series stability test such as gate bias stress, temperature bias stress, negative bias illumination stress and rigorous high temperature/humidity test, it showed significant improvement of reliability. Namely, SU-8 has considerable potential in future passivation application.
In this thesis, we adopted a-IWO nano-sheet, high- dielectric,HfO2 and SU-8 to serve as channel, GI and passivation layer respectively to achieve high performance NSTs with different S/D and different electrical advantages. They are definitely suitable for advanced displays, flexible electronics, three-dimensional integrated circuit (3D-IC) and hybrid-CMOS technologies.