三維積體電路之低溫銅對銅接合技術平台開發
Development of Low Temperature Copper to Copper Bonding Technology Platform for 3D Integrated Circuits
摘要
近年來,由於電晶體的微縮尺寸即將達到物理上的極限,所以半導體行業急需要新的技術來擴展摩爾定律(Moore’s law)、帶動產業進步、提升產能和降低製程成本。三維積體電路技術發展至今,具備以下幾大優勢:縮短RC時間延遲、縮小封裝體積、低功率消耗、低製程成本以及提升系統運行表現。有鑑於此,三維積體電路(3D IC)技術至今仍廣泛的被研究與發展,而接合技術為3D IC中最為關鍵的技術之一,其中最為被廣泛運用的接合技術即為熱壓合(Thermal Compression Bonding, TCB)方法。熱壓合技術一般運用在晶片/晶圓級堆疊(Stacking),主要負責上下層接合導通製程,並以銅為主要內連接之導電材料,實現訊號垂直傳輸的運作。然而,傳統的熱壓接合為了提高接合良率,需要提升接合溫度達攝氏300°C以上,所以在製程溫度上容易造成熱預算過高,進而伴隨各式問題,例如電路性能劣化、對準精度誤差、晶圓翹曲和熱應力殘留等。因此,本論文研究重點將針對三維積體電路之關鍵熱壓合技術的優化進行研究,旨在研發出適合低溫下銅對銅接合的平台,同時期望實現低真空下良好的晶圓級接合品質,並開發出適合在大氣環境下短時間製程的晶片級接合技術。
傳統銅對銅熱壓接合技術需要在高溫高壓的製程條件下進行才能達到較優良的接合品質,但在此環境條件下容易衍生許多問題,所以為了改善此類議題,本論文第一部分,提出一款新型鈍化層材料,作為封蓋式鈍化層(Capping Passivation)方法的研究對象,藉此降低銅對銅接合之製程溫度。從接合測試、材料分析及可靠度測試等結果,本研究已經證實此金屬鈍化層之可行性。接合測試方面,成功完成在120°C,50分鐘下的良好接合。通過穿透式電子顯微鏡分析發現,在低溫下銅原子會藉由鈍化層擴散至表面,形成連續銅膜。因此,可以確定,鈍化層不僅具備防止內部銅氧化之作用,在接合製程當下,亦不會阻擋銅擴散至接合表面,故可實現研究銅對銅接合的目標。另外,通過Kelvin結構進行電性測試,以覆晶接合方式製備,最低製程溫度可到達100°C (3分鐘),最短時間可到達15秒(150°C),兩者皆可通過可靠度測試(2000次的溫度循環測試和264小時的濕度測試),而電阻值結果表現穩定,約為10-7 Ω‧cm2,說明鈍化層結構不受惡劣環境影響,且具備良好結構穩定性。
本論文第二部分,為了進一步開發出超低溫接合製程,研究中加入濕潤層(Wetting Layer)的設計,形成新型鈍化層結構,其總厚度將以超薄膜的基礎為設計,希望此結構可作為一嶄新的低溫接合平台之概念,去實現封蓋式鈍化層技術之開發;其中加入濕潤層的設計,目的在於改善表面薄膜的微結構,使其晶粒變小、表面粗糙度降低,進而實現良好的接合表面。接合測試部分,成功實現在100°C, 15分鐘下高品質接合。且由於金屬鈍化層本身材料的特性,使得該膜層設計不僅具備保護內部銅的功能,還可透過濕潤層的作用,增加表面膜層的晶界數量,進而實現短時間下大量的擴散,因此,不管是對接合條件的溫度、時間,皆可有效的降低至極限,故而成功開發出超低溫接合技術。此研究中,電性測試的樣品以覆晶接合方式製備,最低製程溫度可到達70°C (3分鐘),最短時間可到達15秒(150°C),兩者皆可通過可靠度測試(2000次的溫度循環測試和264小時的濕度測試)。電阻值結果顯示穩定,接觸阻抗與純鈍化層之結果相比較佳,約為10-7~10-8 Ω‧cm2,所以說明新型鈍化層設計結構既不受惡劣環境影響,而且比起純鈍化層更具備良好的接合品質。
本論文透過封蓋式鈍化層方法進行一系列低溫銅對銅接合測試、材料分析及可靠度測試,以銅結構為基底,設計表面鈍化層結構,成功實現低溫對稱晶圓級接合製程,電性量測上阻值皆表現穩定,並通過可靠度測試,證明該論文提出的兩種新型製程概念,皆可提供良好的電性與結構穩定性,對未來TSV間之熱壓接合技術的應用上,將提供良好的改善。此外,為達成業界低製程成本且大量生產的需求,本研究成功實測出以鈍化層結構在大氣環境下,通過覆晶接合方式所能承受的極限溫度(70°C)、極限時間(15秒),並通過可靠度測驗,因此,對未來3D IC異質整合的應用上,可提供良好的接合技術平台。
傳統銅對銅熱壓接合技術需要在高溫高壓的製程條件下進行才能達到較優良的接合品質,但在此環境條件下容易衍生許多問題,所以為了改善此類議題,本論文第一部分,提出一款新型鈍化層材料,作為封蓋式鈍化層(Capping Passivation)方法的研究對象,藉此降低銅對銅接合之製程溫度。從接合測試、材料分析及可靠度測試等結果,本研究已經證實此金屬鈍化層之可行性。接合測試方面,成功完成在120°C,50分鐘下的良好接合。通過穿透式電子顯微鏡分析發現,在低溫下銅原子會藉由鈍化層擴散至表面,形成連續銅膜。因此,可以確定,鈍化層不僅具備防止內部銅氧化之作用,在接合製程當下,亦不會阻擋銅擴散至接合表面,故可實現研究銅對銅接合的目標。另外,通過Kelvin結構進行電性測試,以覆晶接合方式製備,最低製程溫度可到達100°C (3分鐘),最短時間可到達15秒(150°C),兩者皆可通過可靠度測試(2000次的溫度循環測試和264小時的濕度測試),而電阻值結果表現穩定,約為10-7 Ω‧cm2,說明鈍化層結構不受惡劣環境影響,且具備良好結構穩定性。
本論文第二部分,為了進一步開發出超低溫接合製程,研究中加入濕潤層(Wetting Layer)的設計,形成新型鈍化層結構,其總厚度將以超薄膜的基礎為設計,希望此結構可作為一嶄新的低溫接合平台之概念,去實現封蓋式鈍化層技術之開發;其中加入濕潤層的設計,目的在於改善表面薄膜的微結構,使其晶粒變小、表面粗糙度降低,進而實現良好的接合表面。接合測試部分,成功實現在100°C, 15分鐘下高品質接合。且由於金屬鈍化層本身材料的特性,使得該膜層設計不僅具備保護內部銅的功能,還可透過濕潤層的作用,增加表面膜層的晶界數量,進而實現短時間下大量的擴散,因此,不管是對接合條件的溫度、時間,皆可有效的降低至極限,故而成功開發出超低溫接合技術。此研究中,電性測試的樣品以覆晶接合方式製備,最低製程溫度可到達70°C (3分鐘),最短時間可到達15秒(150°C),兩者皆可通過可靠度測試(2000次的溫度循環測試和264小時的濕度測試)。電阻值結果顯示穩定,接觸阻抗與純鈍化層之結果相比較佳,約為10-7~10-8 Ω‧cm2,所以說明新型鈍化層設計結構既不受惡劣環境影響,而且比起純鈍化層更具備良好的接合品質。
本論文透過封蓋式鈍化層方法進行一系列低溫銅對銅接合測試、材料分析及可靠度測試,以銅結構為基底,設計表面鈍化層結構,成功實現低溫對稱晶圓級接合製程,電性量測上阻值皆表現穩定,並通過可靠度測試,證明該論文提出的兩種新型製程概念,皆可提供良好的電性與結構穩定性,對未來TSV間之熱壓接合技術的應用上,將提供良好的改善。此外,為達成業界低製程成本且大量生產的需求,本研究成功實測出以鈍化層結構在大氣環境下,通過覆晶接合方式所能承受的極限溫度(70°C)、極限時間(15秒),並通過可靠度測驗,因此,對未來3D IC異質整合的應用上,可提供良好的接合技術平台。
In recent years, because the shrunk-size of transistors are approaching the physical limits, the semiconductor industry urgently requires some new technologies to expand the Moore’s law, promote the industry progress, increase the production capacity, and reduce process costs. The development of three-dimensional integrated circuit (3D IC) technology has the following advantages: short RC delay, small form factor, low power consumption, low process cost and good system performance. In view of this, 3D IC technology has been widely researched and developed to date, and one of the most important technologies for 3D IC application is the bonding technique. Among the bonding technique, the most widely used method is thermal compression bonding (TCB). The TCB technology is generally utilized as the wafer/chip level stacking process. It is mainly responsible for interconnecting between the upper and lower chip/wafer after bonding process, and the main conduction of the interconnection is through the copper to realize the vertical transmission of signals. However, in order to improve the bonding yield, the conventional TCB needs to raise the bonding temperature more than 300°C. Therefore, it is easy to cause the higher thermal budget in the process, and then it will accompany with various problems, such as the deterioration of circuit performance, the deviation of alignment accuracy, wafer warpage and thermal stress. The focus in this thesis is to study the optimization of the thermal compression bonding technology for 3D integration application, aiming to develop a platform is suitable for copper-to-copper bonding at low temperature and to achieve good quality for wafer-level bonding process under vacuum, and finally, to develop the chip-level bonding methods, which are suitable for short time condition in an atmospheric environment.
The traditional copper-to-copper bonding technology needs to be carried out under the process condition of high temperature and high pressure to realize the good bonding quality, but many problems are easily derived under above environmental condition. In order to improve such issues, the first part of the thesis proposes a new metallic material is utilized in the capping passivation method, thereby reducing the process temperature for the copper-to-copper bonding. From the results of the bonding tests, material analysis and reliability tests, the research has verified the feasibility of the metal passivation layer. For the bonding test, high-quality bonding was successfully completed the bonding process at 120°C for 50 minutes. It was found by transmission electron microscopy (TEM) that copper atoms diffused to the surface through the metal passivation layer, and then it formed a continuous copper layer. Thus, we could confirm that the metal passivation layer not only had the function to prevent internal copper from oxidation, but also did not obstruct the atomic diffusion to the outermost layer during the bonding process. Accordingly, we achieved the goal of the research for the copper-to-copper bonding. In addition, the Kelvin structure was treated as the basic structure for the electrical measurement. The samples were prepared by flip chip bonding. The lowest process temperature was at 100°C (for 3 minutes), and the shortest time was for 15 seconds (at 150°C). Both of them could pass the reliability tests, which were respectively temperature cycling test of 2000 loops and humidity test of 264 hours. The results of contact resistance were stable, which was about 10-7 Ω‧cm2, indicating that the structure for the passivation method was not only unaffected by harsh environment, but also had a good structural stability.
The second part of this thesis is to further develop the bonding process at the ultra-low temperature with the design of the addition of the wetting layer as a new structure for the capping passivation method. The design concept for the wetting layer was to improve the grain size of the thin film deposition, and then obtained a better bonding surface. The bonding test was completed the bonding process at 100 ° C for 15 minutes. Due to the material properties of the metal, the design structure had the function for protecting the internal copper. Besides, the addition of the wetting layer could increase numbers of grain boundaries on the bonding surface, and then it was suitable for the atomic diffusion at low temperature in a short time. Therefore, regardless of the temperature and time for the bonding conditions, they could be effectively reduced to the limit. Undoubtedly, the ultra-low temperature bonding technology had been successfully developed in this research. In this study, the electrical test samples were prepared by flip chip bonding with the lowest process temperature at 70°C (for 3 minutes) and the shortest time for 15 seconds (150°C). Both of them passed the reliability test with temperature cycling test of 2000 loops and humidity test of 264 hours. The contact resistance was stable, and it was lower than the sample with metal passivation, which was about 10-7~10-8 Ω‧cm2. Therefore, the new design structure was not only unaffected by harsh environment, but also had a better bonding quality than metal passivation.
In this thesis, a series of low-temperature copper-to-copper bonding test, material analysis and reliability test are carried out by the capping passivation method. The copper structures with two methods of passivation application are successfully utilized to realize in the symmetric wafer level bonding process at low temperature. The electrical measurements are stable after the reliability test. These results prove that the two process methods proposed in the thesis can provide good performance and structural stability. Therefore, above methods will provide good improvement in the future for the TCB application between TSVs. In addition, in order to achieve the goal such as low cost and high throughput, this study investigates the limit temperature and limit duration time with passivation structure, and the samples are prepared by flip-chip bonding in an atmosphere environment. The above samples already pass the reliability test. In summary, the researches in the thesis provide a platform with the novel bonding technology for the heterogeneous 3D integration and packaging.
The traditional copper-to-copper bonding technology needs to be carried out under the process condition of high temperature and high pressure to realize the good bonding quality, but many problems are easily derived under above environmental condition. In order to improve such issues, the first part of the thesis proposes a new metallic material is utilized in the capping passivation method, thereby reducing the process temperature for the copper-to-copper bonding. From the results of the bonding tests, material analysis and reliability tests, the research has verified the feasibility of the metal passivation layer. For the bonding test, high-quality bonding was successfully completed the bonding process at 120°C for 50 minutes. It was found by transmission electron microscopy (TEM) that copper atoms diffused to the surface through the metal passivation layer, and then it formed a continuous copper layer. Thus, we could confirm that the metal passivation layer not only had the function to prevent internal copper from oxidation, but also did not obstruct the atomic diffusion to the outermost layer during the bonding process. Accordingly, we achieved the goal of the research for the copper-to-copper bonding. In addition, the Kelvin structure was treated as the basic structure for the electrical measurement. The samples were prepared by flip chip bonding. The lowest process temperature was at 100°C (for 3 minutes), and the shortest time was for 15 seconds (at 150°C). Both of them could pass the reliability tests, which were respectively temperature cycling test of 2000 loops and humidity test of 264 hours. The results of contact resistance were stable, which was about 10-7 Ω‧cm2, indicating that the structure for the passivation method was not only unaffected by harsh environment, but also had a good structural stability.
The second part of this thesis is to further develop the bonding process at the ultra-low temperature with the design of the addition of the wetting layer as a new structure for the capping passivation method. The design concept for the wetting layer was to improve the grain size of the thin film deposition, and then obtained a better bonding surface. The bonding test was completed the bonding process at 100 ° C for 15 minutes. Due to the material properties of the metal, the design structure had the function for protecting the internal copper. Besides, the addition of the wetting layer could increase numbers of grain boundaries on the bonding surface, and then it was suitable for the atomic diffusion at low temperature in a short time. Therefore, regardless of the temperature and time for the bonding conditions, they could be effectively reduced to the limit. Undoubtedly, the ultra-low temperature bonding technology had been successfully developed in this research. In this study, the electrical test samples were prepared by flip chip bonding with the lowest process temperature at 70°C (for 3 minutes) and the shortest time for 15 seconds (150°C). Both of them passed the reliability test with temperature cycling test of 2000 loops and humidity test of 264 hours. The contact resistance was stable, and it was lower than the sample with metal passivation, which was about 10-7~10-8 Ω‧cm2. Therefore, the new design structure was not only unaffected by harsh environment, but also had a better bonding quality than metal passivation.
In this thesis, a series of low-temperature copper-to-copper bonding test, material analysis and reliability test are carried out by the capping passivation method. The copper structures with two methods of passivation application are successfully utilized to realize in the symmetric wafer level bonding process at low temperature. The electrical measurements are stable after the reliability test. These results prove that the two process methods proposed in the thesis can provide good performance and structural stability. Therefore, above methods will provide good improvement in the future for the TCB application between TSVs. In addition, in order to achieve the goal such as low cost and high throughput, this study investigates the limit temperature and limit duration time with passivation structure, and the samples are prepared by flip-chip bonding in an atmosphere environment. The above samples already pass the reliability test. In summary, the researches in the thesis provide a platform with the novel bonding technology for the heterogeneous 3D integration and packaging.