水質對水錶腐蝕與積垢之影響:批次實驗模擬

Effects of water quality on corrosion and scaling of the water meter by batch simulation test

檔案

全文未公開。

日期

2019

類型

語言

中文

摘要

05年台灣自來水公司發現用戶水錶有積垢情形發生,內部積垢的累積可能會使水錶計量不準確,影響用水計量。積垢生成與水錶腐蝕而溶出金屬沉積有關,且各地區水錶積垢嚴重程度也隨著設置段水質而有所異同。故本研究為釐清水質對水錶腐蝕與積垢生成之關聯性,以新竹市自來水為基質,個別配製不同濃度的含次氯酸鈉、硫酸鈣及鹼度之自來水進行水錶切片(黃銅鑄件)的浸泡試驗。另以燒杯與離心管浸泡試驗模擬管線半滿管與滿管情況,探討空氣存在對水錶腐蝕與積垢之影響。
研究結果顯示,浸泡含高濃度氯離子之自來水的水錶切片(黃銅鑄件),會有最高的腐蝕滲透速率與促進效率(0.15 mpy與69.7%),且會導致最大的腐蝕與積垢面積生成(9.88π及34.6 mm2)。次之為含高濃度硫酸鈣之自來水(0.13 mpy及65.1%),其腐蝕與積垢面積分別為(6.61π及21.3 mm2)。氯離子或硫酸鈣濃度越高,其腐蝕與積垢程度越嚴重。反之水中鹼度越高,水錶切片(黃銅鑄件)腐蝕與積垢生成會受到抑制;空氣對腐蝕與積垢影響並不顯著。腐蝕與積垢有著密不可分的關係,在特定水質環境中如氯離子或鈣離子及硫酸鹽越高,會有較明顯的腐蝕與積垢生成。腐蝕反應先行發生,導致金屬溶出的問題,並依照不同水質環境有不同的腐蝕型態,積垢生成則伴隨著腐蝕型態,即積垢為腐蝕行為後所留下的結果。
The existence of scaling in the water meter suspected to the outcome of corrosion was found to adversely affect the usage of tap water. The sediments (scaling) accumulated in water meters could not only decrease the amount of water distributed to the household but also induce inaccurate measurement of water meter. It was known that the severity of corrosion and scaling in different area can be various due to the inconsistent of water quality. Therefore, this study aimed to clarify the effects of water quality on corrosion and scaling of the water meter by batch simulation test. The experiment was conducted by immersing yellow brass of the water meter into the tap water. Sodium hypochlorite, calcium sulfate and sodium bicarbonate were introduced respectively into each of the sample for the soaking test. Simultaneously, the soaking test was separated into the beaker and the centrifuge tube soaking test to simulate the condition of half full tube and full tube in the real pipeline systems.
The result showed that the highest corrosion penetration rate (0.15 mpy) and promotion efficiency (69.7%) were detected when yellow brass exposed to high concentration of chloride. Moreover, the largest corrosion (9.88π) and scaling area (34.6 mm2) were also obtained. However, the amount of calcium or sulfate existed in the water presented a slightly minor impact on not only the corrosion penetration rate (0.13 mpy) and promotion efficiency (65.1%), but also on the corrosion (6.61π) and scaling area (21.3 mm2). On the other hand, apparent alleviation of corrosion and scale formation were observed when the alkalinity of the water was higher. The effect of air exposure showed insignificant differences on corrosion and scale formation of the sliced water meter.
In addition, corrosion and fouling are closely connected and inseparable. In certain water environments, such as the significant evidence of chloride or calcium ion and sulfate, there will cause obvious corrosion and scaling. The corrosion reaction occurs first, causing the problem of metal dissolution, and then it is produced according to different water quality. The formation of scale is accompanied by the corrosion pattern, that is, the result of corrosion.

所屬典藏

環境工程研究所
顯示完整詮釋資料 統計資料

引用此條目

曾治寰 (2019). 水質對水錶腐蝕與積垢之影響:批次實驗模擬. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/72121

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/72121