摘要

本研究利用平均破壞時間(Mean-time-to-failure,MTTF)測試搭配修正的Black方程式分析鍺銻碲單晶奈米線(Ge2Sb2Te5 Nanowires,GST NWs)在脈衝偏壓環境下的電遷移(Electromigration,EM)行為,探討脈衝峰值電流密度(jp)、占空比(d)、頻率(f)及溫度(T)等參數對GST NWs的EM行為之影響。
GST NWs係利用氣液固相法製備,並以X光繞射儀、掃描式電子顯微鏡(Scaning Electron Microscopy,SEM)及能量散佈分析儀(Energy Dispersive Spectroscopy,EDS)、穿隧式電子顯微鏡等分析GST NWs的形貌、結構和組成。
在脈衝偏壓環境的MTTF測試顯示,f大於10 MHz時,GST NWs的EM行為可利用平均電流模型描述;200°C、不同jp範圍之MTTF量測顯示電流密度加速因子(n)約為1.01,此意味著表面擴散為EM破壞之主導機制;不同溫度的MTTF分析顯示EM活化能為1.38 eV,高於GST NWs在直流偏壓測試所得之1.23 eV,表示GST NWs在脈衝偏壓環境的抗EM破壞能力較佳。EDS分析顯示在EM過程中,GST NWs中的Te原子朝陽極端遷移,Ge與Sb原子則往陰極端方向遷移;SEM分析發現在EM破壞末期GST NWs之陰極端會形成局部頸縮,此顯示電子風力主導EM過程之質流遷移,推斷局部頸縮應為表面擴散造成空位累積所致,凹口區之電流密度提升使得焦耳熱效應增強,進而導致GST NWs之EM破壞。
This study performs the mean-time-to-failure (MTTF) tests under pulse bias environment to evaluate the electromigration (EM) behaviors of Ge2Sb2Te5 nanowires (GST NWs). The modified Black’s equation was adopted for EM analysis and the parameters under investigation included the peak current density (jp), the duty cycle (d) and the frequency (f) of pulse bias as well as the temperature (T) of test environment.
GST NWs were synthesized by the vapor-liquid-solid method. Afterward, their morphology, microstructure and compositions were analyzed by x-ray diffraction, scanning electron microscopy (SEM), energy dispersive sectroscopy (EDS).
The MTTF tests under pluse bias found that the EM behaviors of GST NWs can be depicted by the average current model when f > 10 MHz. The MTTF tests performed at 200°C and various jp ranges indicated that the current density exponent of Black’s equation (n) is about equal to 1.01, implying the dominance of surface diffusion for the mass transport of EM process. Moreover, the MTTF tests performed at various temperatures revealed that the activation energy of EM is about 1.38 eV. This implied a better resistance to EM failure for GST NWs under pulse bias in comparison with GST samples under DC bias. EDS analysis indicated that the Te elements migrate to the anode side whereas the Ge and Sb elements move to the cathode side of GST NWs subjected to the pulse bias. SEM observed the occurrence of necking in cathode side of GST NWs when EM failure occurred. This indicated the electron wind force effect dominates the mass transport during EM process. The necking is ascribed to the vacancy accumulation caused by the surface diffusion, consequently escalating the Joule heating effect and eventually leading to the failure of GST NWs.
顯示完整詮釋資料 統計資料

引用此條目

羅劭恩 (2019). 製備鍺銻碲單晶奈米線及其在脈衝偏壓環境之電遷移行為研究. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/73591