直流反應濺鍍氮化鈦於單晶鑽石(100)之異質磊晶成長
Heteroepitaxial Growth of Titanium Nitride on Single Crystalline Diamond (100) by DC Reactive Sputtering
摘要
氮化鈦(Titanium Nitride, TiN) 具有岩鹽(rock salt)型之面心立方晶體結構,且具有高硬度、高熔點、低電阻率、高化學安定性、高耐磨耗性、低摩擦係數等性質,而鑽石具有優異之半導體性質,TiN磊晶薄膜可應用於鑽石半導體元件之電極。本論文將探討以直流反應磁控濺鍍法(DC reactive magnetron sputtering)沉積磊晶之製程,並成功地在單晶鑽石基板上沉積TiN磊晶薄膜。薄膜的量測與分析之技術包括原子力顯微鏡(Atomic Force Microscopy, AFM)、X光繞射(X-Ray Diffraction, XRD)、X光電子能譜(X-ray photoelectron spectroscopy, XPS)、掃描式電子顯微鏡(Scanning Electron Microscopy, SEM)、四點探針(Four-Point Probe)與掃描穿透式電子顯微鏡(Scanning Transmission Electron Microscopy, STEM)等,藉此了解TiN磊晶薄膜結晶在各製程條件下其薄膜微結構、結晶品質與性質之變化,進而探究磊晶薄膜形成之機制。
在本論文中,濺鍍薄膜成長之機台設定溫度(nominaltemperature)為870C,其他主要的濺鍍製程參數,包括N2與Ar氣體混合比例(2.5 – 10% N2)、功率(40 – 60 W)及製程壓力(0.467 - 0.6 Pa),其中又以N2比例影響最為明顯。XRD分析結果顯示,濺鍍於Diamond (100)基板的TiN磊晶薄膜之品質,以(002) X光搖擺曲線半高寬量測,可達到1.12°,電阻率 32 4 μΩ cm。XRD φ掃描結果和TEM分析顯示得知TiN薄膜與Diamod (100)基板之間的磊晶關係為TiN (001) ∥ Diamond (100);TiN [110] ∥ Diamod [110]。XPS分析顯示,N與Ti之比例接近1/1。AFM結果顯示表面,粗糙度為2.4 nm。
在本論文中,濺鍍薄膜成長之機台設定溫度(nominaltemperature)為870C,其他主要的濺鍍製程參數,包括N2與Ar氣體混合比例(2.5 – 10% N2)、功率(40 – 60 W)及製程壓力(0.467 - 0.6 Pa),其中又以N2比例影響最為明顯。XRD分析結果顯示,濺鍍於Diamond (100)基板的TiN磊晶薄膜之品質,以(002) X光搖擺曲線半高寬量測,可達到1.12°,電阻率 32 4 μΩ cm。XRD φ掃描結果和TEM分析顯示得知TiN薄膜與Diamod (100)基板之間的磊晶關係為TiN (001) ∥ Diamond (100);TiN [110] ∥ Diamod [110]。XPS分析顯示,N與Ti之比例接近1/1。AFM結果顯示表面,粗糙度為2.4 nm。
TiN of rock salt structure posseses many excellent properties such as high electrical conductivity, high hardness, and thigh themal stability with chemical inertness, which can be applied on diamond semiconductor devices as electrode for high temperature and high power conditions. This thesis mainly explores the deposition condition for epitaxial TiN growth on diamond (100) by reactive DC magnetron sputtering. Film characterization with epitaxial qualities in terms of crystallinity, microstructure, surface morphology, stoichiometry, and resistivity was performed by using x-ray diffraction (XRD) scanning transmission electron microscopy (STEM), scanning Electron Microscopy (SEM), x-ray photoelectron spectroscopy (XPS), and four-point probe.
The various sputtering conditions for TiN film growth at nominl temperature of 870C have been done including gas mixture of N2/Ar ratio ranging from 2.5 to 10%, power (40 – 60 W), and work pressure (0.467 - 0.6 Pa). The results show that the TiN film grown on diamond with 7.5% N2 in Ar at 60 W is of high quality with the lowest full width at half maximum (FWHM) of 1.12° for (002) x-ray rocking curve (XRC) and reisitivity of 32 μΩ cm. The X-ray φ-scan results also show that TiN is in epitaxy with diamond (100) in the epitaxial relationship of TiN (100) // diamond (100) and TiN [011] // diamond [011]. XPS depth profiles show the stoichiometric ratio of Ti and N is close to 1. The surface roughness of the TiN film measured by AFM was 2.4 nm. Cross-sectional TEM in atomic resolution shows the TiN is in epitaxy with diamond across the interface.
The various sputtering conditions for TiN film growth at nominl temperature of 870C have been done including gas mixture of N2/Ar ratio ranging from 2.5 to 10%, power (40 – 60 W), and work pressure (0.467 - 0.6 Pa). The results show that the TiN film grown on diamond with 7.5% N2 in Ar at 60 W is of high quality with the lowest full width at half maximum (FWHM) of 1.12° for (002) x-ray rocking curve (XRC) and reisitivity of 32 μΩ cm. The X-ray φ-scan results also show that TiN is in epitaxy with diamond (100) in the epitaxial relationship of TiN (100) // diamond (100) and TiN [011] // diamond [011]. XPS depth profiles show the stoichiometric ratio of Ti and N is close to 1. The surface roughness of the TiN film measured by AFM was 2.4 nm. Cross-sectional TEM in atomic resolution shows the TiN is in epitaxy with diamond across the interface.