利用環境無害的水溶液法製備氧化銦薄膜電晶體

Fabrication of In2O3-based Thin Film Transistors via an Environment-Friendly Aqueous Route

檔案

日期

2020

類型

語言

中文

摘要

本研究使用對環境無害的水溶液法製作氧化銦(Indium Oxide,In2O3)薄膜,並探討不同硬烤溫度對於氧化銦薄膜電晶體(Thin-film Transistor,TFT)電性的影響。
本實驗以In2O3作為TFT通道層。首先利用接觸角量測儀測量基板親水性,找出最佳的表面前處理參數。接著針對In2O3薄膜進行材料分析,其中包括以掃描式電子顯微鏡與原子力顯微鏡觀察薄膜表面型態,X光繞射(X-ray Diffraction,XRD)分析薄膜晶體結構,X光光電子能譜儀(X-ray Photoelectron Spectroscopy,XPS)分析薄膜組成及霍爾效應儀分析半導體基本物理性質。最後以鉬(Molybdenum,Mo)為上電極,以製成In2O3-TFT元件,並分析元件特性。
本實驗以硝酸銦為前驅物,將其加入去離子水攪拌一小時後,取適量旋轉塗佈於SiO2(250 nm)/Si基板上。經100C軟烤與200至300C硬烤後,XRD分析顯示可得到非晶相、連續性In2O3薄膜。XPS分析顯示In2O3薄膜的氧缺陷比例隨硬烤溫度升高由40.0% 下降至24.6%;霍爾效應儀量測顯示In2O3薄膜的載子濃度約為1014 cm3,硬烤溫度的影響不大,霍爾遷移率(Hall Mobility,Hall)則隨硬烤溫度提高而增加,此意味著高硬烤溫度能改善In的ns軌域重疊排列之週期性且降低載子在傳輸過程之缺陷散射程度。
In2O3薄膜製備完成後,以磁控濺度方式於In2O3薄膜上方鍍上Mo電極,完成底閘極式In2O3-TFT的製備。實驗結果顯示,含經250C硬烤之In2O3通道層的TFT元件具有最佳之電性質。在汲極電壓為20 V時,其臨界電壓為0.02 V、次臨界擺幅為2.6 V/decade、開關電流比為104及飽和載子遷移率為1.9 cm2/Vsec。
This study presents an environment-friendly method for the preparation of amorphous indium oxide (In2O3) thin film and the investigation of the relationship between annealing temperature and electrical properties of In2O3-based thin film transistors (TFTs). For In2O3 thin film preparation, indium nitrate hydrate (In(NO3)3·xH2O) was used as the precursor and deionized water was used as solvent. After spin-coating the solution on SiO2/Si substrates, the samples were annealed at 200 to 300C so as to form the continuous In2O3 thin films. Afterward, the In2O3 thin films were analyzed by scanning electron microscopy and atomic force microscopy for the film morphology, x-ray diffraction for the crystallinity, x-ray photoelectron spectroscopy (XPS) for the chemical status and Hall effect measurement for fundamental semiconductor properties. Finally, we fabricated the In2O3-based TFT devices and measured their transport characteristics.
XPS analysis revealed that the fraction of oxygen defects in In2O3 thin films decreases from 40.0% to 24.6% when annealing temperature increases from 200 to 300C. Hall effect measurement showed that the carrier concentrations are about 1014 cm3 for all In2O3 thin films and the annealing temperature has no significant effect. However, the Hall mobility increased with the increase of annealing temperature, implying the improvement of ns orbital overlap and the suppression of scattering effects during carrier transport. The TFT device containing In2O3 active channel layer annealed at 250C exhibited the best electrical performance with the on/off current ratio greater than 104, the saturation mobility of 1.9 cm2/Vsec, the substhreshold swing of 2.6 V/decade and the threshold voltage of 0.02 V.
顯示完整詮釋資料 統計資料

引用此條目

蔡語萱 (2020). 利用環境無害的水溶液法製備氧化銦薄膜電晶體. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/76252

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。