扇形柱狀晶奈米雙晶銅之電鍍與微結構分析
Electrodeposition and Microstructure Examination of the Radiating Columnar Nanotwinned Copper
摘要
目前工業界主要是以電鍍沉積進行銅薄膜的製作,此種銅薄膜的結晶大多為多晶無優選方向的結構,一般具有高延伸率(> 15%)和低抗拉強度(< 400MPa)的物理性質。而本實驗採用一種特殊配方的添加劑,搭配最為廣泛應用的直流電鍍法,即可沉積出具有柱狀奈米雙晶銅薄膜,相較於一般無優選方向的多晶銅,奈米雙晶銅擁有更高的抗拉強度(500 - 800MPa)、以及更優秀的抗電遷移能力、熱穩定性、硬度、抗氧化能力等、並能延緩金屬疲勞的時間。
本實驗主要目的為探討一種新型態扇形柱狀晶結構奈米雙晶銅的形成原因。首先利用直流電或脈衝電流沉積奈米雙晶銅後,再以離子研磨機(Ion Milling)切蝕出待觀察的鍍層橫切面,最後用冷場發射式電子顯微鏡(Field Emission Scanning Electron Microscopes, FE-SEM)及背向散射電子繞射分析儀(Electron Backscattered Diffraction, EBSD)分析其微結構。
在銅離子濃度相同的情況下,使用不同電流密度之直流電電鍍,隨著電流密度升高,原本垂直成長的奈米雙晶銅柱狀晶會逐漸往兩旁傾斜,呈現扇子張開狀向四周發散,經EBSD分析,原<111>優選方向的奈米雙晶銅將由92.2%降低至31.6%。
若將直流電改為脈衝電流來製備奈米雙晶銅,以週期性地開啟電流(on)-關閉電流(off)反覆施加於被鍍物,發現電流關閉的時間一旦延長,容易成長垂直的柱狀晶。經EBSD分析,<111>優選方向的奈米雙晶銅則會由31.6%增加至99.8%。
此外,若先以不同電流密度在極短時間下製備一層奈米雙晶銅薄膜,可發現其表面粗糙度(Surface Roughness)會隨著電流密度而改變,接著再用固定相同的電流密度繼續沉積奈米雙晶銅,會發現在不同表面粗糙度的晶種層上,後續沉積奈米雙晶銅的扇形柱狀晶比例也不相同,實驗發現,若表面粗糙度越大,微結構中扇形柱狀晶結構奈米雙晶銅的比例就越高。
本實驗主要目的為探討一種新型態扇形柱狀晶結構奈米雙晶銅的形成原因。首先利用直流電或脈衝電流沉積奈米雙晶銅後,再以離子研磨機(Ion Milling)切蝕出待觀察的鍍層橫切面,最後用冷場發射式電子顯微鏡(Field Emission Scanning Electron Microscopes, FE-SEM)及背向散射電子繞射分析儀(Electron Backscattered Diffraction, EBSD)分析其微結構。
在銅離子濃度相同的情況下,使用不同電流密度之直流電電鍍,隨著電流密度升高,原本垂直成長的奈米雙晶銅柱狀晶會逐漸往兩旁傾斜,呈現扇子張開狀向四周發散,經EBSD分析,原<111>優選方向的奈米雙晶銅將由92.2%降低至31.6%。
若將直流電改為脈衝電流來製備奈米雙晶銅,以週期性地開啟電流(on)-關閉電流(off)反覆施加於被鍍物,發現電流關閉的時間一旦延長,容易成長垂直的柱狀晶。經EBSD分析,<111>優選方向的奈米雙晶銅則會由31.6%增加至99.8%。
此外,若先以不同電流密度在極短時間下製備一層奈米雙晶銅薄膜,可發現其表面粗糙度(Surface Roughness)會隨著電流密度而改變,接著再用固定相同的電流密度繼續沉積奈米雙晶銅,會發現在不同表面粗糙度的晶種層上,後續沉積奈米雙晶銅的扇形柱狀晶比例也不相同,實驗發現,若表面粗糙度越大,微結構中扇形柱狀晶結構奈米雙晶銅的比例就越高。
Nowadays, the copper metallization is usually implemented by electrod-eposition, which usually produces randomly-oriented grains. A high elongation (>15%) and a low tensile strength (<400MPa) are intrinsic to this microstructure. In this study, a proprietary formula was used along with direct current (DC) plating to deposit the columnar nanotwinned copper (nt-Cu) films. Compared with the randomly-oriented structure, the nt-Cu possesses many advantages, including higher tensile strength (500~800MPa), electromigration resistance, thermal stability, hardness, anti-oxidation ability, as well as superior fatigue performance.
The purpose of this study is to investigate the mechanism of a novel radiating columnar nt-Cu. The nt-Cu film is formed by direct current or pulsed current plating. The microstructure is examined by Field Emission Scanning Electron Microscopes (FE-SEM) equipped with Electron Backscattered Diffraction (EBSD).
The vertical columnar grains grew inclined gradually as the current density of DC plating increased as the copper ion concentration remained the same. Moreover, the inclined columnar grains radiated from the nuclei during deposition, forming a fan-like structure. It was proved by EBSD that the dominating <111> orientation dropped dramatically from 92.2% to only 31.6% when the radiating columnar grains presented.
When pulsed plating was used, in which the current was applied on and off repeatedly, a longer off-time facilitates the growth of the vertical columnar (111)-oriented grains. EBSD showed the <111> orientation rose from 31.6% to 99.8%.
In addition, effect of surface roughness of the Cu seed on the growth of the nt-Cu films was also studied. It was found that the surface roughness can affect the growth of radiating column grains. As the surface roughness increases, the percentage of radiating column grains increases. However, with a smooth Cu seed layer, vertical (111)-oriented grains prevails.
The purpose of this study is to investigate the mechanism of a novel radiating columnar nt-Cu. The nt-Cu film is formed by direct current or pulsed current plating. The microstructure is examined by Field Emission Scanning Electron Microscopes (FE-SEM) equipped with Electron Backscattered Diffraction (EBSD).
The vertical columnar grains grew inclined gradually as the current density of DC plating increased as the copper ion concentration remained the same. Moreover, the inclined columnar grains radiated from the nuclei during deposition, forming a fan-like structure. It was proved by EBSD that the dominating <111> orientation dropped dramatically from 92.2% to only 31.6% when the radiating columnar grains presented.
When pulsed plating was used, in which the current was applied on and off repeatedly, a longer off-time facilitates the growth of the vertical columnar (111)-oriented grains. EBSD showed the <111> orientation rose from 31.6% to 99.8%.
In addition, effect of surface roughness of the Cu seed on the growth of the nt-Cu films was also studied. It was found that the surface roughness can affect the growth of radiating column grains. As the surface roughness increases, the percentage of radiating column grains increases. However, with a smooth Cu seed layer, vertical (111)-oriented grains prevails.