少數層二硒化鈀之電性傳輸與熱電性質
Electric transport and thermoelectric properties in few-layer PdSe2
摘要
尋找高效率的熱電材料是一個重要而有趣的課題,二維 (Two-Dimensional, 2D) 過渡金屬二硫化合物 (Transition Metal Dichalcogenides, TMDC),因其優越的熱電性能以及未來廣闊的應用前景而受到廣泛關注。其中,二維二硒化鈀 (PdSe2) 因其理論上計算出高熱電性能,吸引了眾多科研工作者的目光。
本實驗使用機械剝離法,剝取少數層PdSe2,利用半導體製程技術製作少數層二硒化鈀的場效電晶體與熱電元件,在室溫下研究了二硒化鈀的電性。本實驗中,二硒化鈀為n型半導體材料,電流的開關比 (On/Off Ratio) 約爲104,臨界擺幅 (Subthreshold Swing, S.S.) 約爲9.52 V/dec,載流子遷移率 (Mobility) 最大為34.7 cm2·V-1·S-1。 另外,在二硒化鈀元件的熱電性能測量上,得到的最大席貝克係數約爲655 µV/K,與理論值十分接近,並觀察到席貝克值與電晶體場效應有關聯性。當閘極偏壓設定在臨界電壓附近時,席貝克係數到達峰值,而當閘極偏壓小於臨界電壓時,通道關閉沒有熱電效應。
最後計算了二硒化鈀的熱電功率因子(Power Factor, PF),通過調節閘極偏壓觀察熱電功率因子隨場效應的變化,並對比相應的材料層數,發現最大熱電功率因子為0.26 mW/m·K2,材料厚度為12層,證明二硒化鈀是極具潛力的熱電材料。
本實驗使用機械剝離法,剝取少數層PdSe2,利用半導體製程技術製作少數層二硒化鈀的場效電晶體與熱電元件,在室溫下研究了二硒化鈀的電性。本實驗中,二硒化鈀為n型半導體材料,電流的開關比 (On/Off Ratio) 約爲104,臨界擺幅 (Subthreshold Swing, S.S.) 約爲9.52 V/dec,載流子遷移率 (Mobility) 最大為34.7 cm2·V-1·S-1。 另外,在二硒化鈀元件的熱電性能測量上,得到的最大席貝克係數約爲655 µV/K,與理論值十分接近,並觀察到席貝克值與電晶體場效應有關聯性。當閘極偏壓設定在臨界電壓附近時,席貝克係數到達峰值,而當閘極偏壓小於臨界電壓時,通道關閉沒有熱電效應。
最後計算了二硒化鈀的熱電功率因子(Power Factor, PF),通過調節閘極偏壓觀察熱電功率因子隨場效應的變化,並對比相應的材料層數,發現最大熱電功率因子為0.26 mW/m·K2,材料厚度為12層,證明二硒化鈀是極具潛力的熱電材料。
The search of high-efficiency thermoelectric materials is always an important and interesting topic. Two-dimensional (2D) transition metal dichalcogenides (TMDC) have received extensive attention due to their superior thermoelectric properties and broad application prospects in the future. Among them, PdSe2 has shown outstanding thermoelectric properties according to theoretical calculations.
Here we employed mechanical exfoliation to peel off few layers PdSe2, flakes from the bulk and we adopted standard e-beam lithography and thermal evaporation to fabricate field-effect transistors (FET) and thermodynamic devices based on few-layer PdSe2 flakes. The field-effect electrical properties of PdSe2 flakes were studied at room temperature. It was found that PdSe2 is an n-type semiconductor material. The on/off ratio of the PdSe2 FET is about 104 and the subthreshold swing (SS) is about 9.52 V/dec. Its maximum carrier mobility is about 34.7 cm2·V-1·S-1.
The thermoelectric performance of the PdSe2 element is obtained and the maximum Seebeck coefficient is about 655 µV/K which is very close to the theoretical calculation. In addition, a correlation between the Seebeck value and the field effect properties is observed. When the gate bias voltage is set close to the threshold voltage, the Seebeck coefficient reaches its peak value. On the other hand, the thermoelectric effect is reduced if the gate bias voltage is tuned to be lower than the threshold voltage.
Finally, the thermoelectric power factor (PF) of PdSe2 is estimated. By adjusting the gate bias voltage, the change of thermoelectric PF following the field effect is observed. It is found that the maximum power factor is about 0.26 mW/m·K2 for the PbSe2 flake with a thickness of 12 layers, implying it to be a promising thermoelectric material.
Here we employed mechanical exfoliation to peel off few layers PdSe2, flakes from the bulk and we adopted standard e-beam lithography and thermal evaporation to fabricate field-effect transistors (FET) and thermodynamic devices based on few-layer PdSe2 flakes. The field-effect electrical properties of PdSe2 flakes were studied at room temperature. It was found that PdSe2 is an n-type semiconductor material. The on/off ratio of the PdSe2 FET is about 104 and the subthreshold swing (SS) is about 9.52 V/dec. Its maximum carrier mobility is about 34.7 cm2·V-1·S-1.
The thermoelectric performance of the PdSe2 element is obtained and the maximum Seebeck coefficient is about 655 µV/K which is very close to the theoretical calculation. In addition, a correlation between the Seebeck value and the field effect properties is observed. When the gate bias voltage is set close to the threshold voltage, the Seebeck coefficient reaches its peak value. On the other hand, the thermoelectric effect is reduced if the gate bias voltage is tuned to be lower than the threshold voltage.
Finally, the thermoelectric power factor (PF) of PdSe2 is estimated. By adjusting the gate bias voltage, the change of thermoelectric PF following the field effect is observed. It is found that the maximum power factor is about 0.26 mW/m·K2 for the PbSe2 flake with a thickness of 12 layers, implying it to be a promising thermoelectric material.