以鋁摻雜及氨電漿處理對矽鍺通道材料介面品質之研究
Study on the Interface Properties of SiGe Channel Using NH3 Plasma Treatment With Al Doping
摘要
本篇論文中,我們使用原子層沉積系統(ALD)中氨電漿對矽鍺介面進行氮化處理,並將氨電漿的結果對比鋁摻雜和氨電漿處理疊加的效果,以降低介面層中氧化鍺的含量作為研究主軸,希望藉此提升介面品質。
首先,我們透過X射線光電子能譜學(XPS)對矽鍺(Si0.8Ge0.2)基板之介面層進行材料分析,其結果顯示,使用單純氨電漿處理於矽鍺基板上,介面層中存在氧化鍺的訊號,而使用鋁摻雜氨電漿的方式,氧化鍺的訊號被有效降低,表示介面層中幾乎沒有鍺氧鍵結。此外,透過沉積二氧化鉿於介面層上形成閘極堆疊的電容製作,其電性量測結果呈現出減少氧化層中氧化鍺的含量,可以有效降低介面能態密度(Dit)到1.41×1012 cm-2eV-1。然而穿透式電子顯微鏡(TEM)的分析結果顯示鋁摻雜會形成較厚的介面層,進而造成等效閘極氧化層(EOT)變厚。我們嘗試進行縮薄氧化層厚度的實驗,但積累電容值仍無法有效提升,這是因為在不充足的氨電漿環境下會造成介面處有較高比例的氧化鍺形成。
我們成功於矽鍺(Si0.8Ge0.2)基板上製作出P型的金氧半場效應電晶體,透過鋁摻雜和充足的氨電漿處理於介面層,可以有效的降低次臨界擺幅(S.S.),並且能提升汲極電流開關比達到6.06×106。此外,矽鍺金氧半場效應電晶體的導通電流和電洞的等效遷移率都能獲得提升,這是源自於有效改善介面缺陷電荷,使得載子在矽鍺通道的傳輸過程中受到較小的庫倫散射所致。
首先,我們透過X射線光電子能譜學(XPS)對矽鍺(Si0.8Ge0.2)基板之介面層進行材料分析,其結果顯示,使用單純氨電漿處理於矽鍺基板上,介面層中存在氧化鍺的訊號,而使用鋁摻雜氨電漿的方式,氧化鍺的訊號被有效降低,表示介面層中幾乎沒有鍺氧鍵結。此外,透過沉積二氧化鉿於介面層上形成閘極堆疊的電容製作,其電性量測結果呈現出減少氧化層中氧化鍺的含量,可以有效降低介面能態密度(Dit)到1.41×1012 cm-2eV-1。然而穿透式電子顯微鏡(TEM)的分析結果顯示鋁摻雜會形成較厚的介面層,進而造成等效閘極氧化層(EOT)變厚。我們嘗試進行縮薄氧化層厚度的實驗,但積累電容值仍無法有效提升,這是因為在不充足的氨電漿環境下會造成介面處有較高比例的氧化鍺形成。
我們成功於矽鍺(Si0.8Ge0.2)基板上製作出P型的金氧半場效應電晶體,透過鋁摻雜和充足的氨電漿處理於介面層,可以有效的降低次臨界擺幅(S.S.),並且能提升汲極電流開關比達到6.06×106。此外,矽鍺金氧半場效應電晶體的導通電流和電洞的等效遷移率都能獲得提升,這是源自於有效改善介面缺陷電荷,使得載子在矽鍺通道的傳輸過程中受到較小的庫倫散射所致。
In this thesis, we utilized NH3 plasma treatment in the ALD system to process nitridation on the SiGe interface. The comparison of the results of NH3 plasma treatment with TMA-doped NH3 plasma-treated on IL was executed to testify the effect of Al-doping. Our research spindle is to reduce the content of GeOx to improve the interfacial quality.
We firstly conducted material analysis on the interfacial layer of SiGe substrates by XPS. The XPS analysis of Ge 2p core level shows the GeO peak existed in IL treated by NH3 plasma. The GeO peak could be effectively lowered down by excessive TMA treatment, indicating that there is almost no Ge-O bonding in the interfacial layer. In addition, the SiGe gate stack was formed by depositing HfO2 on IL for the fabrication of MOSCAPs. From the measurements of MOSCAPs, the value of Dit could be improved to 1.41×1012 cm-2eV-1 due to the reduction of GeOx. However, the TEM results displayed that thicker IL was formed by using excessive TMA treatment, bringing about the increase of EOT. We tried to scale down the thickness of IL, but encountered limitations on enhancing the value of Cacc since insufficient NH3 plasma treatment would lead to a higher concentration of GeOx.
Finally, we successfully fabricated Si0.8Ge0.2 p-MOSFETs with IL formed by various deposition conditions. By Al doping and adequate NH3 plasma treatment, the value of S.S. was significantly decreased, and the Ion/Ioff ratio of ID could be improved to 6.06×106. Besides, the on-current and effective hole mobility were improved due to the interface states which could trap the charge to interfere hole transport in the channel were ameliorated and induce less coulomb scattering.
We firstly conducted material analysis on the interfacial layer of SiGe substrates by XPS. The XPS analysis of Ge 2p core level shows the GeO peak existed in IL treated by NH3 plasma. The GeO peak could be effectively lowered down by excessive TMA treatment, indicating that there is almost no Ge-O bonding in the interfacial layer. In addition, the SiGe gate stack was formed by depositing HfO2 on IL for the fabrication of MOSCAPs. From the measurements of MOSCAPs, the value of Dit could be improved to 1.41×1012 cm-2eV-1 due to the reduction of GeOx. However, the TEM results displayed that thicker IL was formed by using excessive TMA treatment, bringing about the increase of EOT. We tried to scale down the thickness of IL, but encountered limitations on enhancing the value of Cacc since insufficient NH3 plasma treatment would lead to a higher concentration of GeOx.
Finally, we successfully fabricated Si0.8Ge0.2 p-MOSFETs with IL formed by various deposition conditions. By Al doping and adequate NH3 plasma treatment, the value of S.S. was significantly decreased, and the Ion/Ioff ratio of ID could be improved to 6.06×106. Besides, the on-current and effective hole mobility were improved due to the interface states which could trap the charge to interfere hole transport in the channel were ameliorated and induce less coulomb scattering.