建築結構高強度螺栓於火害後殘餘機械性質之研究

Residual Mechanical Properties of Post-Fire Structural High Strength Bolts

檔案

日期

2022

類型

語言

中文

摘要

鋼構造建築對於火害的抵抗能力偏低,其原因為鋼材與連接用的螺栓易在高溫作用與冷卻方式下導致其殘餘機械性質變化並進而影響鋼結構之強度。目前國內對於高強度螺栓在不同火場溫度與冷卻方式下的殘餘機械性質變化了解甚少,故本研究將探討高強度螺栓於火害後其殘餘性質變化。研究方法為將常用之高強度螺栓加熱至200oC與1000oC間,以空氣冷卻或水中冷卻等方式進行冷卻,爾後進行拉伸試驗以建立各項火害後螺栓之殘餘機械性質。
在加熱溫度500oC前,加熱溫度與冷卻方式對各項殘餘機械性質皆不造成明顯影響。在加熱溫度500oC至700oC間,冷卻方式與加熱溫度影響並不顯著,F10T系列螺栓之降伏強度與抗拉強度相較常溫試體皆顯著下降。在加熱溫度700oC以上,加熱溫度與冷卻方式將對F10T系列螺栓之殘餘機械性質產生大幅影響。以空氣冷卻之試體,降伏強度與抗拉強度明顯低於常溫試體,其伸長率與延性較常溫試體顯著上升;置於水中冷卻之試體,降伏強度與抗拉強度明顯高於常溫試體,其伸長率與延性較常溫試體顯著下降。置於水中冷卻之試體,彈性模數與常溫試體並無明顯差異,並無觀察到隨溫度改變之變化趨勢。在加熱溫度700oC前,以空氣冷卻試體之彈性模數與常溫試體無異;在加熱溫度700oC後,彈性模數略為下降並在加熱溫度達1000℃時恢復至略低於常溫試體。
在加熱溫度700oC前,無論何種冷卻方式,試體韌性與常溫試體並無顯著差異;在加熱溫度700oC後,以空氣冷卻試體之韌性在略為上升後下降,以水中冷卻試體之韌性高於常溫試體,脆性破壞試體除外。在加熱溫度700oC前,無論何種冷卻方式,F10T系列螺栓皆為韌性破壞,其斷面皆有明顯之頸縮現象。在加熱溫度700oC以上,以空氣冷卻之螺栓皆仍為韌性破壞;以水中冷卻之螺栓有部分試體出現脆性破壞。
Steel structure lacks the ability of fire resistance. Due to the effects of high temperature and cooling methods, the steel plates and bolts will change their residual mechanical properties and then affect the strength of the steel structure. So far, the research on residual mechanical properties of high-strength bolts under different temperatures and cooling methods in Taiwan is limited. Therefore, a series of experimental studies about post-fire, high-strength bolts was conducted to investigate their residual mechanical properties. High-strength bolts were heated to specific temperatures and then cooled in air or water. Tension tests were performed for cooled bolts, and the residual mechanical properties of the high-strength bolt were established based on the test results.
The residual mechanical properties of F10T series high-strength bolts heated under 500oC were not affected significantly by different temperature and cooling methods. When the bolts were heated between 500oC and 700oC, regardless of temperature and cooling methods, the yield strength and tensile strength of F10T series high-strength bolts dropped significantly. When the bolts were heated above 700oC, the residual mechanical properties of F10T series high-strength bolts were affected significantly by the temperature and cooling methods. For bolts cooled in water, compared with those in ambient temperature, the yield strength and tensile strength rose significantly, and the elongation and ductility dropped significantly. For bolts cooled in air, compared with those in ambient temperature, the yield strength and tensile strength dropped significantly, and the elongation and ductility rose significantly. Regardless of the variation in temperature, the elastic modulus of bolts cooled in water did not change significantly compared with bolts in ambient temperature. When the bolts were heated under 700oC, there was a little difference in elastic modulus between the bolts in ambient temperature and the bolts cooled in air. When the bolts were heated above 700oC, the elastic modulus dropped slightly and then recovered when they were heated to 1000oC.
Regardless of cooling methods, there was little difference in toughness between the bolts in ambient temperature and the bolts heated under 700oC. When the bolts were heated above 700oC, the toughness of bolts cooled in air rose slightly and then dropped. When the bolts were heated above 700oC, the toughness of bolts cooled in water was higher than bolts in ambient temperature, except for bolts that experienced brittle failure. Regardless of cooling methods, when the bolts were heated under 700oC, F10T series high-strength bolts experienced ductile failure with necking in the fracture surface, and no brittle failure occurred. When the bolts were heated above 700oC, most bolts experienced ductile failure, except for several bolts cooled in water that experienced brittle failure.

所屬典藏

土木工程學系
顯示完整詮釋資料 統計資料

引用此條目

趙俊宇 (2022). 建築結構高強度螺栓於火害後殘餘機械性質之研究. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/81057

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/81057