TiC為岩鹽(rock-salt)型結構,具備高硬度、高熔點、高熱穩定性、導電性佳等優異性質。本研究中將以反應式磁控濺鍍(reactive magnetron sputtering)沉積磊晶TiC薄膜於Si (100)基板上,而後以微波電漿氮化法對TiC薄膜進行氮化。後續使用微波電漿化學氣相沉積法(microwave plasma chemical vapor deposition)沉積鑽石薄膜於TiC緩衝層上。本論文可分為兩部分,第一部分主要探討反應式磁控濺鍍磊晶TiC薄膜並將其氮化,探討反應氣體比例、製程時間、製程壓力間的影響,並研究薄膜與基板間的磊晶關係、界面情況與反應形成之機制。第二部分則注重於改變偏壓條件,探討微波電漿化學氣相沉積鑽石於TiC/Si (100)之成核狀況,並嘗試成長鑽石薄膜。
第一部分以反應式磁控濺鍍並使用Ti靶材與CH4/Ar混合氣體,於Si (100)基板上成長磊晶TiC薄膜,基板溫度設定於650C並探討CH4比例、製程時間、製程壓力對薄膜性質的影響,CH4比例本研究將針對3、4、5%進行測試,製程壓力則為2 × 10-3、3 × 10-3 Torr進行沉積,製程時間分別為10、15 min。而後以微波電漿針對TiC薄膜進行氮化,通入N2/H2作為反應氣體,N2比例固定於99%。探討製程壓力、製程時間對薄膜氮化之影響。本研究中設定製程壓力於30、40 Torr,製程時間1、2 h。X光繞射(X-ray diffraction, XRD)、穿透式電子顯微鏡(transmission electron microscopy, TEM)與掃描穿透式電子顯微鏡(scanning transmission electron microscopy, STEM)顯示,本研究成功沉積品質良好之磊晶TiC (100)薄膜於Si (100)基板上,其磊晶關係為TiC (100)[0¯11]∥Si (100)[0¯11]。晶格以晶域匹配磊晶(domain match expitaxy)形成,比例為5/4。當甲烷比例為4%、製程壓力3 × 10-3 Torr、製程時間10 min時,其X光搖擺曲線(X-ray rocking curve, XRC)之半高寬(full width at half maximum, FWHM)為1.24、電阻約為90 μΩ·cm。XPS結果顯示薄膜內部[C]/[Ti]原子比例趨近於1且界面處有SiC生成。氮化部分結果顯示,於製程壓力40 Torr、製程時間2 h的條件下,TiC薄膜受電漿氮化表面組成接近於TiN,且氮化層TiCxN1-x與TiC及Si基板依然呈現磊晶關係:TiCxN1-x (100)[0¯11]∥TiC (100)[0¯11]∥Si (100)[0¯11]。氮化所產生之XRD繞射訊號TiCxN1-x,其搖擺曲線之半高寬為0.618。XPS結果顯示,N原子經由擴散不斷向TiC薄膜內部躍遷,其濃度隨距離而呈現指數型遞減,使薄膜組成產生漸變的現象,直到靠近Si基板其組成為TiC0.9N0.1。
第二部分為鑽石於TiC/Si基板上沉積的研究,TiC/Si試片透過積碳與偏壓輔助成核法(bias-enhanced nucleation, BEN),使TiC薄膜表面產生足夠密度的鑽石核種,並進行後續的成長。在BEN階段中嘗試以改良之環狀上電極,在上電極為+ 200 V偏壓條件,以不同的製程參數,CH4比例為2、3、5%,製程壓力為20、30 Torr,製程時間為5、15分鐘,製程功率600、800 W,進行試驗。探討其對鑽石核種密度之影響並嘗試將其成長為連續膜。透過掃描式電子顯微鏡(scanning electron microscopy, SEM)對鑽石進行表面形貌分析,並透過拉曼光譜儀(Raman spectroscopy)確認鑽石核種的存在與結晶品質。實驗結果顯示,經1 h積碳後於5% CH4 比例進行5分鐘的BEN,其鑽石密度可達1.6 × 109 /cm2。
第一部分以反應式磁控濺鍍並使用Ti靶材與CH4/Ar混合氣體,於Si (100)基板上成長磊晶TiC薄膜,基板溫度設定於650C並探討CH4比例、製程時間、製程壓力對薄膜性質的影響,CH4比例本研究將針對3、4、5%進行測試,製程壓力則為2 × 10-3、3 × 10-3 Torr進行沉積,製程時間分別為10、15 min。而後以微波電漿針對TiC薄膜進行氮化,通入N2/H2作為反應氣體,N2比例固定於99%。探討製程壓力、製程時間對薄膜氮化之影響。本研究中設定製程壓力於30、40 Torr,製程時間1、2 h。X光繞射(X-ray diffraction, XRD)、穿透式電子顯微鏡(transmission electron microscopy, TEM)與掃描穿透式電子顯微鏡(scanning transmission electron microscopy, STEM)顯示,本研究成功沉積品質良好之磊晶TiC (100)薄膜於Si (100)基板上,其磊晶關係為TiC (100)[0¯11]∥Si (100)[0¯11]。晶格以晶域匹配磊晶(domain match expitaxy)形成,比例為5/4。當甲烷比例為4%、製程壓力3 × 10-3 Torr、製程時間10 min時,其X光搖擺曲線(X-ray rocking curve, XRC)之半高寬(full width at half maximum, FWHM)為1.24、電阻約為90 μΩ·cm。XPS結果顯示薄膜內部[C]/[Ti]原子比例趨近於1且界面處有SiC生成。氮化部分結果顯示,於製程壓力40 Torr、製程時間2 h的條件下,TiC薄膜受電漿氮化表面組成接近於TiN,且氮化層TiCxN1-x與TiC及Si基板依然呈現磊晶關係:TiCxN1-x (100)[0¯11]∥TiC (100)[0¯11]∥Si (100)[0¯11]。氮化所產生之XRD繞射訊號TiCxN1-x,其搖擺曲線之半高寬為0.618。XPS結果顯示,N原子經由擴散不斷向TiC薄膜內部躍遷,其濃度隨距離而呈現指數型遞減,使薄膜組成產生漸變的現象,直到靠近Si基板其組成為TiC0.9N0.1。
第二部分為鑽石於TiC/Si基板上沉積的研究,TiC/Si試片透過積碳與偏壓輔助成核法(bias-enhanced nucleation, BEN),使TiC薄膜表面產生足夠密度的鑽石核種,並進行後續的成長。在BEN階段中嘗試以改良之環狀上電極,在上電極為+ 200 V偏壓條件,以不同的製程參數,CH4比例為2、3、5%,製程壓力為20、30 Torr,製程時間為5、15分鐘,製程功率600、800 W,進行試驗。探討其對鑽石核種密度之影響並嘗試將其成長為連續膜。透過掃描式電子顯微鏡(scanning electron microscopy, SEM)對鑽石進行表面形貌分析,並透過拉曼光譜儀(Raman spectroscopy)確認鑽石核種的存在與結晶品質。實驗結果顯示,經1 h積碳後於5% CH4 比例進行5分鐘的BEN,其鑽石密度可達1.6 × 109 /cm2。
TiC has a rock-salt structure, and has many extraordinary properties such as high hardness, high melting point, high thermal stability, and good electrical conductivity. This research focuses on deposition of buffer layer for diamond film growth on (100) Si substrate by using reactively magnetron sputtered epitaxial TiC and plasma nitridation of TiC film. The thesis is divided into two parts. First, reactive magnetron sputtering deposition of epitaxial TiC on Si (100) and plasma nitridation of the TiC film are investigated through the influence of reactive gas flow ratio, deposition time and process pressure. Also, the epitaxial relationship between TiC and Si, interfacial reaction and mechanism are studied. In the second part, bias-enhanced nucleation (BEN) of diamond in microwave plasma chemical vapor deposition (MPCVD) and diamond growth are carried out.
For the TiC film growth, reactive magnetron sputtering is done with 2-inch Ti target and gas mixture of CH4 and H2. Substrate temperature is set at 650C. The sputtering condition is varied as following: CH4 in Ar from 3 to 5%, process pressure at 2 × 10-3 and 3 × 10-3 Torr, process time for 10 and 15 min. Plasma nitridation of the deposited TiC film is done with the plamas of 1% H2 in N2 at 30 and 40 Torr for 1 and 2 h. The results from X-ray diffraction (XRD), transmission electron microscopy (TEM) and scanning transmission electron electron microscopy (STEM) show that epitaxial cubic TiC of high quality is grown on Si by domain match epitaxy in 5/4 ratio with the epitaxial relationship of TiC (100)[0¯11]∥Si (100)[0¯11].For sputtering conditions of 4% CH4, 3 × 10-3 Torr and 10 min, the TiC film has an full width at half maximum (FWHM) of 200 X-ray rocking curve (XRC) of 1.24 with the electrical resistivity of 90 μΩ·cm。The result of XPS reveals that the atomic ratio of Ti to C is close to 1 in the film, and SiC phase exists at the interface. The result from the nitrided TiC film under 40 Torr for 2 h indicates that the film composition near the surface region is almost fully nitrided with Ti/N atomic ratio close to 1. The nitrided TiCxN1-x still remains in epitaxy with TiC and Si in the relationship of TiCxN1-x (100)[0¯11]∥TiC (100)[0¯11]∥Si (100)[0¯11]。The full width at half maximum of (200) TiCxN1-x XRC can be reduced to 0.618.The result of XPS shows that N atoms diffuse through the TiC film and the N concentration decreases exponentially with the distance. The film composition close to the substrate is determined to be TiC0.9N0.1.
The second part for diamond deposition on the TiC/Si susbtrate, BEN which is performed with a ring-shaped upper anode (+ 200 V) after caburization for 1 hour is applied for diamond nucleation on the TiC film. The variation of the diamond nucleation density with the BEN condition is investigated in terms of CH4 flow ratio, pressure, time, and power. Scanning electron microscopy is used to analyze the morphology of the diamond film. Also, Raman spectroscopy is used to verify the existence and quality of diamond nuclei. It is observed that the diamond nucleation density can reach 1.6 × 109 /cm2.
For the TiC film growth, reactive magnetron sputtering is done with 2-inch Ti target and gas mixture of CH4 and H2. Substrate temperature is set at 650C. The sputtering condition is varied as following: CH4 in Ar from 3 to 5%, process pressure at 2 × 10-3 and 3 × 10-3 Torr, process time for 10 and 15 min. Plasma nitridation of the deposited TiC film is done with the plamas of 1% H2 in N2 at 30 and 40 Torr for 1 and 2 h. The results from X-ray diffraction (XRD), transmission electron microscopy (TEM) and scanning transmission electron electron microscopy (STEM) show that epitaxial cubic TiC of high quality is grown on Si by domain match epitaxy in 5/4 ratio with the epitaxial relationship of TiC (100)[0¯11]∥Si (100)[0¯11].For sputtering conditions of 4% CH4, 3 × 10-3 Torr and 10 min, the TiC film has an full width at half maximum (FWHM) of 200 X-ray rocking curve (XRC) of 1.24 with the electrical resistivity of 90 μΩ·cm。The result of XPS reveals that the atomic ratio of Ti to C is close to 1 in the film, and SiC phase exists at the interface. The result from the nitrided TiC film under 40 Torr for 2 h indicates that the film composition near the surface region is almost fully nitrided with Ti/N atomic ratio close to 1. The nitrided TiCxN1-x still remains in epitaxy with TiC and Si in the relationship of TiCxN1-x (100)[0¯11]∥TiC (100)[0¯11]∥Si (100)[0¯11]。The full width at half maximum of (200) TiCxN1-x XRC can be reduced to 0.618.The result of XPS shows that N atoms diffuse through the TiC film and the N concentration decreases exponentially with the distance. The film composition close to the substrate is determined to be TiC0.9N0.1.
The second part for diamond deposition on the TiC/Si susbtrate, BEN which is performed with a ring-shaped upper anode (+ 200 V) after caburization for 1 hour is applied for diamond nucleation on the TiC film. The variation of the diamond nucleation density with the BEN condition is investigated in terms of CH4 flow ratio, pressure, time, and power. Scanning electron microscopy is used to analyze the morphology of the diamond film. Also, Raman spectroscopy is used to verify the existence and quality of diamond nuclei. It is observed that the diamond nucleation density can reach 1.6 × 109 /cm2.