反應濺鍍 (111) TiC磊晶薄膜於(0001) 4H-SiC晶片之製備及其應用於方向性鑽石膜成長之研究

Reactive Sputtering Deposition of Epitaxial TiC (111) Buffer Layer on 4H-SiC (0001) and its Application for Oriented Diamond Growth

檔案

日期

2022

類型

語言

中文

摘要

本研究致力於以微波化學氣相沉積法(Microwave Plasma Chemical Vapor Deposition, MPCVD)沉積方向性鑽石膜於4H-SiC (0001)基板上,並於沉積鑽石前以直流反應式磁控濺鍍(Reactive Direct Current Magnetron Sputtering, R-DCMS)沉積磊晶TiC (111)薄膜於4H-SiC(0001)基板上,作為緩衝層。本論文可分為兩部分,第一部分探討反應式濺鍍TiC磊晶薄膜,改變CH4比例及沉積時間,研究薄膜磊晶品質、化學組成、界面情況、微結構分析。第二部分為探討沉積方向性鑽石膜,依照沉積步驟積碳、偏壓成核、成長三個步驟分別討論微波功率、CH4比例、製程時間、製程壓力對於鑽石成核、成長於TiC (111)/4H-SiC (0001)上之情形。
第一部分使用直流反應式磁控濺鍍,濺射靶材為2吋Ti金屬靶、通入氣體為CH4/Ar混合氣體、基板加熱溫度為670 C、直流功率固定為50 W,探討改變CH4比例、濺鍍時間對於TiC薄膜性質之影響。CH4比例針對3、4、5、6 %進行實驗、沉積時間則選擇7分鐘及15分鐘。X光繞射(XRD)顯示以CH4比例4 % 所製備之TiC薄膜具有較佳結晶品質,其X光搖擺曲線(XRC)之半高寬約為140 arcsec,而膜厚約88 nm、表面粗糙度(Rq)為1.07 nm、電阻率約為81 μΩ‧cm。由XRC結果與穿透式電子顯微鏡(TEM)及掃描穿透式電子顯微鏡(STEM)影像互相比對,證實TiC薄膜之臨界厚度約為70 nm,當膜厚超過臨界厚度時會因應立釋放而產生分層現象,臨界厚度內為仍受應力影響、結晶品質較佳之應力層;超過臨界厚度則為應力釋放、結晶品質下降之釋放層。XRD ϕ scan及STEM ADF影像證實TiC與4H-SiC具有磊晶關係,且TiC薄膜內包含雙晶特徵,磊晶關係為TiC (111) // 4H-SiC (0001)及TiC [1 ̅10] // 4H-SiC [112 ̅0] (TiC [11 ̅0] // 4H-SiC [112 ̅0]為雙晶中另一方向)。X光光電子能譜儀(XPS)分析結果顯示TiC薄膜內組成單一且均勻,同時也不受結晶品質改變影響。
第二部分利用微波電漿化學氣相沉積法於TiC (111)/4H-SiC (0001)沉積鑽石膜。透過積碳、偏壓輔助成核法(Bias-Enhanced Nucleation, BEN)兩階段製程可於導電TiC薄膜表面沉積足夠密度之核種,以利後續鑽石膜成長。積碳及偏壓成核階段會額外使用環狀上電極裝置,並改變微波功率、CH4比例、偏壓時間探討其對於核種之影響。掃描式電子顯微鏡(SEM)影像所有實驗參數中,核種密度最高可達1.9  109 cm-2,平均核種粒徑大小為70 nm,而拉曼光譜結果顯示所沉積之核種並非由鑽石相單一組成,其中仍包含D-band及G-band等其他鍵結。以上述條件所沉積之核種進行成長,改變CH4比例、製程壓力、成長時間探討其對於鑽石膜成長之影響。經連續成長10小時後,於SEM影像中可以發現鑽石膜主要由三角形晶面組成,其平均邊長為2.55 μm,但並不具有統一之方向性,膜厚約3.9 μm;而拉曼光譜結果呈現明顯鑽石訊號,其峰值為1334.10 cm-1、半高寬為13.42 cm-1,顯示鑽石膜具有一定結晶品質且呈受壓應力。XRD結果顯示所沉積之鑽石膜為(111)方向性多晶鑽石膜。
This work focuses on deposition of oriented diamond film on TiC/4H-SiC (0001) substrate by using microwave plasma chemical vapor deposition (MPCVD). The TiC buffer layer on the 4H-SiC substrate was epitaxially grown by reactive sputtering before diamond deposition. This thesis is divided into two parts. The first part studies the reactive magnetron sputtering deposition conditions of epitaxial (111) TiC on 4H-SiC with different reactive gas flow ratios and different deposition times. Film properties including crystalline quality, epitaxial relationship, chemical composition and microstructure are also investigated to understand the effect of reactive sputtering conditions. In the second part, the deposition of oriented diamond films is investigated through different microwave power, CH4 flow ratio, process pressure and process time in each deposition step as carburization, bias-enhanced nucleation (BEN), and growth.
In the first part, reactive sputtering is performed using a 2-inch Ti target and CH4/Ar mixed gas. The substrate temperature was maintained at approximately 670 °C and the DC power was fixed at 50 W. The CH4 flow ratio is varied from 3 to 6 % and the deposition time are 7 and 15 min. The results from X-ray diffraction (XRD) show that the TiC film deposited with 4 % CH4 flow ratio for 15 min has better crystalline quality as shown with (111) x-ray rocking curve (XRC) full width at half-maximum (FWHM) of ~ 140 arcsec and the resistivity of 81 μΩ‧cm. The film thickness is nearly 90 nm and the surface roughness (Rq) is 1.01 nm. The results from XRC, transmission electron microscopy (TEM) and scanning TEM (STEM) prove that there exists a critical thickness of TiC film of approximately 70 nm above which the relaxation of film stress occurs. The bottom layer (< 70 nm) remains stressed and retains good crystalline quality, while the top layer above the critical thickness is relaxed with deteriorated crystalline quality. XRD ϕ scan results and STEM annular dark field (ADF) images reveal the epitaxial relationship between TiC film and 4H-SiC substrate with the epitaxial relationship of TiC (111) // 4H-SiC (0001) and TiC [1 ̅10] // 4H-SiC [112 ̅0]. In addition, the twin structure is oberseved in the epitaxial TiC film with TiC (111) // 4H-SiC (0001) and TiC [11 ̅0] // 4H-SiC [112 ̅0]. XPS results show that the [C]/[Ti] atomic ratio in the TiC film is close to 1 through the whole film thickness.
The second part is the deposition of (111) oriented diamond film on TiC/4H-SiC by using MPCVD. Through the two-step process of carburization and BEN, a sufficient nucleation density can be obtained on the surface of the conductive TiC film to facilitate subsequent film growth. For BEN, a ring-shaped upper anode is additionally used, and the processing condition is changed by varying the microwave power, CH4 flow ratio, and process time to explore the effects on nucleation. Scanning electron microscopy (SEM) images show that the nucleation density can reach 1.9  109 cm-2 with average crystal size 70 nm. However, Raman spectra reaveal that there is not only diamond phase in the nucleations, but also D-band and G-band carbon phases. The subsequent growth is performed with different CH4 flow ratio, process pressure, and process time. After growth for10 hours, the surface morphology of the grown diamond film consists of triangular facets with side lengths of 2.55 μm without apparently preferred orinetation. The thickness of the diamond film is approximate 3.9 μm. In the Raman spectra, the diamond peak at 1334.10 cm-1 with FWHM of 13.42 cm-1 indicates that the diamond film has a reasonably good crystallinity and is under compressive stress. XRD results show that the diamond film is polycrystalline and (111) oriented.
顯示完整詮釋資料 統計資料

引用此條目

林靖峰 (2022). 反應濺鍍 (111) TiC磊晶薄膜於(0001) 4H-SiC晶片之製備及其應用於方向性鑽石膜成長之研究. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/82080

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/82080