摘要

This work focuses on deposition of highly oriented diamond (HOD) film on
conductive n-type 4H-SiC (0001) substrate. The diamond deposition is performed by
microwave plasma chemical vapor deposition (MPCVD).This thesis is divided into
two parts. The first part studies bias-enhanced nucleation (BEN) on 4H-SiC (0001)
substrate. In the second part, growth of diamond were carried out to obtain a (111)
HOD film on the 4H-SiC (0001).
For the diamond nucleation on C-face 4H-SiC, a ring-shaped upper anode was
used for applying the bias voltage. The increase on the nucleation density was
explored by varying the BEN conditions including CH4 concentration and bais time.
Scanning electron microscopy (SEM) observations show that the nucleation density
generally increases with increasing CH4 concentration and bias time. The density can
reach 1 x 109 cm-2 after BEN at + 200 V for a short period of 3 min. However, if the
bias time is too long, secondary nucleation will occur.
To further grow of a (111) highly oriented diamond film, the influence of
different process conditions on the diamond film is presented. The SEM results show
that the methane concentration lower than 0.3% is favorable for formation of (111)
diamond facets, but after long time growth pyramid-like diamonds are easily formed
with a rough surface and the diamond film is prone to peel off. In order to improve
such a situation, a two-step method for growth was developed. The first step is fast
growth preferably along <111> by using a low methane concentration, followed by
increasing methane concentration in the second step to switch the growth direction along <100>. As a result, a relatively smooth surface of the diamond film is
obtained. The results of Raman spectroscopy show that the full width at half
maximum (FWHM) of the diamond peak is about 13 cm-1, suggesting the film of
good crystallinity with insignificantly residual stress. SEM characterization shows
that the proportion of identifiable (111) diamonds reaches more than 90%. X-ray
diffraction analysis shows the evidence of the (111) highly oriented diamond film
from the strong diamond (111) diffraction peak intensity.
本論文主要研究以微波電漿化學氣相沉積進行高方向性(111)鑽石沉積, 第
一部份主要探討偏壓輔助成核法在具導電性之 n 型 4H-SiC 基板上進行鑽石的成
核的最佳參數,第二部份以不同的成長條件沉積高方向性(111)鑽石膜,並分析
鑽石成長在 SiC 上之特徵。
在成核部份,以環形上電極加上+ 200 V 偏壓, 進行直流偏壓增強成核法
(bias-enhanced nucleation, BEN)於具導電性之 n 型 4H-SiC 之碳面上進行偏壓, 並
分析不同的製程條件對於成核結果的影響, 由實驗結果得知較高的甲烷濃度與較
長的偏壓時間有助於成核密度的提升,但偏壓時間過長容易導致二次成核的發生,
對於後續方向性鑽石膜的成長較為不利。 以掃描式電子顯微鏡(SEM)進行分析,
結果顯示以該方式進行成核後鑽石核種的密度可達到 1 x 109 cm-2 以上。
第二部份為成長高方向性(111)鑽石膜, 以第一部分成核參數為基礎,探討不
同製程條件對於鑽石膜的影響, 由 SEM 的分析顯示以較低的甲烷濃度< 0.3% 進
行鑽石膜成長較易形成(111)鑽石晶面, 但在長時間成長後容易形成角錐形鑽石,
造成表面不平整,並且容易出現鑽石膜剝離的現象; 為了改善此一現象,改以二
階段的方式作成長,第一階段先以鑽石縱向成長沿<111>方向為主,第二階段變
更甲烷濃度,鑽石以側向成長為主, 增加<100>方向之成長速率,而使{100}消失,
以該方式進行成長後,改善了鑽石膜表面不平整的情況,拉曼光譜分析的結果顯
示鑽石訊號峰之半高寬約 13 cm-1, 具有良好的結晶品質, 鑽石膜受應力影響小,SEM 分析顯示可辨識的(111)鑽石比例達到 90%以上, XRD 分析顯示鑽石(111)
繞射強度高,鑽石膜的晶面以(111)為主, 積分強度 I111/I220 > 4,具有(111)織構(優
選取向), 成功以直流偏壓增強成核法直接在 4H-SiC 基板上成長出具高方向性
(111)鑽石薄膜。
顯示完整詮釋資料 統計資料

引用此條目

梁聖杰 (2022). 偏壓輔助成核法於 n 型 4H-SiC(0001)基板上之高方向性 (111)鑽石膜成核及成長. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/82147

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/82147