全溶液製程混成式電阻式記憶體之研製

Investigation and Fabrication of All-Solution Process Hybrid Resistive Memory Device

檔案

全文未公開。

日期

2023

類型

語言

中文

摘要

本研究首先以聚甲基丙烯酸甲酯(Poly(methyl methacrylate);PMMA)溶液以不同旋塗轉速及溶劑製備薄膜元件,後將材料與四種不同鎂摻雜濃度的氧化鋅奈米粒子混成製作中間層,作為變因以尋求最佳參數。實驗結果以2000rpm溶劑為丙酮的PMMA溶液製成之電阻式記憶體展現最佳特性,其元件結構為氧化銦錫/PMMA/鋁,具有1025次開關循環次數、2.33×10^3的開關電流比,寫入/抹除電壓分別為-0.74 V/ 0.38 V,記憶保持時間達 12000 秒,預估壽命可達10^5秒以上。
考慮到鹽酸多巴胺材料具有更好的附著力及生物相容性,故改採以鹽酸多巴胺溶液製成電阻式記憶體。 其中以濃度為50 mg/ml且轉速為1000 rpm,並以銀漆作為上電極的多巴胺元件具有最佳的記憶特性,其元件結構為氧化銦錫/鹽酸多巴胺/銀漆,具有543次開關循環次數、7.63×10^2的開關電流比,寫入/抹除電壓分別為-0.94 V/ 0.92 V,記憶保持時間達 12000 秒,預估壽命可達106秒以上。
這些結果說明全溶液製程所製備的多巴胺元件不只具有較優異的記憶特性,更因製程過程簡單快速、低成本且無汙染等優勢,展現了其在電阻式記憶體方面的潛力。
In this study, we first prepared thin film devices with Poly(methyl methacrylate) (PMMA) solutions at different spin coating speeds and solvents. Subsequently, the materials were mixed with MgZnO nanoparticles with different Mg doping concentrations to form an intermediate layer, in order to investigate the optimal parameters. Experimental results showed that the PMMA film, prepared at 2000 rpm using acetone as the solvent, exhibited the best characteristics for resistive memory devices. The device structure comprised of indium tin oxide ITO/ PMMA/ Al, demonstrating 1025 switching cycles, the ON/OFF current ratio could be up to 2.33×10^3, write/erase voltages were -0.74 V/0.38 V, the memory retention time of 12000 seconds, and the estimated lifetime could be up to 10^5 s.
Considering the superior adhesion properties and biocompatibility of dopamine materials in hydrochloric acid solution, we used dopamine as the intermediate layer for the fabrication of resistive memory devices. Among various conditions, the dopamine-based device prepared with a concentration of 50 mg/ml and a spin coating speed of 1000 rpm, with silver paste as the top electrode, exhibited the best memory characteristics. The device structure consisted of ITO/ Dopamine Hydrochloride/ Silver Paint, demonstrated switching cycle of 543 times, the ON/OFF current ratio reached 7.63×10^2, write/erase voltages were -0.94 V/0.92 V, the memory retention time could be up to 12000 seconds, and the estimated lifetime could exceed 10^6 s.
These results demonstrated that the Dopamine-based devices fabricated by the all solution-process not only exhibit superior memory characteristics but also possess advantages such as a simple, fast, low-cost, and contamination-free fabrication process, manifested their potential in resistive memory applications.

所屬典藏

光電系統研究所
顯示完整詮釋資料 統計資料

引用此條目

陳嬿亘 (2023). 全溶液製程混成式電阻式記憶體之研製. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/83708

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/83708