可應用於先進封裝與超細間距之具金屬鈍化層輔助低溫鈷對鈷接合技術研究
Investigation of Low-temperature Co-Co Bonding with Metal Passivation for Advanced Packaging and Ultra-Fine Pitch Applications
摘要
本論文提出使用鈷替代銅作為接合材料,並分別搭配銀與銀合金作為鈍化層,探討其在低溫條件下的接合潛力。鈷具備較短的電子平均自由路徑與優異的抗電遷移能力,特別適合應用於小線寬與高可靠度需求的先進封裝領域。但鈷同樣容易氧化且在低溫條件下擴散能力有限,因此本研究透過鍍上金屬鈍化層的方式,降低氧化風險並促進接合界面原子擴散,以達成低溫下的高品質金屬接合。
首先針對鈷對鈷接合搭配10 奈米銀鈍化層之低溫接合行為進行初步驗證,評估其接合品質與電性表現,並與未使用鈍化層的結構進行對比。實驗結果顯示,銀鈍化層可有效降低鈷表面粗糙度並改善接合品質,使接合溫度可降至150 °C仍具備良好機械強度(>5 MPa),在200 °C時即達到低於10⁻⁷ Ω·cm²的接觸電阻,展現優異的導電特性。
接著,再進一步優化鈍化結構,分別探討使用銀合金與減薄至3 奈米的銀鈍化層之接合表現。實驗結果顯示,使用銀合金作為鈍化層之結構接合強度優於純銀結構,且即使在150 °C下仍可維持導通特性,於低溫條件下也具備穩定的導電行為。另一方面,將銀鈍化層厚度減薄至3 奈米後,也可於150 °C下實現接合,其接觸電阻仍維持在10⁻⁷ Ω·cm²等級,展現了不亞於銀合金之導電能力。
最後透過X射線光電子能譜(XPS)與穿透式電子顯微鏡(TEM)等材料分析方式,進一步釐清上述鈍化結構於熱處理後的元素擴散行為與接合介面形貌。XPS縱深分析顯示,銀與銀合金皆能有效抑制氧化並促進鈷原子擴散;其中,3 奈米銀結構的擴散程度最為顯著。TEM影像顯示銀合金結構於接合後形成較穩定且連續的介面,團聚現象相對較少,有助於提升機械與導電表現。不過,觀察結果亦指出,銀合金薄膜與理想情況相比仍出現了局部團聚現象。根據XPS分析,銀合金鈍化層結構表現出較高的氧訊號,而氧的存在可能降低銀表面能,導致銀或合金中銀成分在局部位置產生重組與團聚。此外,銀合金薄膜的初始粗糙度偏高,也會進一步促使局部結構晶粒成長。儘管如此,其團聚程度明顯低於純銀結構,整體仍維持良好之接合完整性,進一步驗證其具潛力的接合強度與應用價值。
經過驗證,本研究系統性展示搭配金屬鈍化層的鈷對鈷低溫接合結構,在不需高溫的情況下即可實現優異的機械與電性整合,並成功應用於晶圓與晶片層級,為未來高密度先進封裝與三維積體電路應用中,提供一項具備技術潛力與實務可行性的金屬接合解決方案。
首先針對鈷對鈷接合搭配10 奈米銀鈍化層之低溫接合行為進行初步驗證,評估其接合品質與電性表現,並與未使用鈍化層的結構進行對比。實驗結果顯示,銀鈍化層可有效降低鈷表面粗糙度並改善接合品質,使接合溫度可降至150 °C仍具備良好機械強度(>5 MPa),在200 °C時即達到低於10⁻⁷ Ω·cm²的接觸電阻,展現優異的導電特性。
接著,再進一步優化鈍化結構,分別探討使用銀合金與減薄至3 奈米的銀鈍化層之接合表現。實驗結果顯示,使用銀合金作為鈍化層之結構接合強度優於純銀結構,且即使在150 °C下仍可維持導通特性,於低溫條件下也具備穩定的導電行為。另一方面,將銀鈍化層厚度減薄至3 奈米後,也可於150 °C下實現接合,其接觸電阻仍維持在10⁻⁷ Ω·cm²等級,展現了不亞於銀合金之導電能力。
最後透過X射線光電子能譜(XPS)與穿透式電子顯微鏡(TEM)等材料分析方式,進一步釐清上述鈍化結構於熱處理後的元素擴散行為與接合介面形貌。XPS縱深分析顯示,銀與銀合金皆能有效抑制氧化並促進鈷原子擴散;其中,3 奈米銀結構的擴散程度最為顯著。TEM影像顯示銀合金結構於接合後形成較穩定且連續的介面,團聚現象相對較少,有助於提升機械與導電表現。不過,觀察結果亦指出,銀合金薄膜與理想情況相比仍出現了局部團聚現象。根據XPS分析,銀合金鈍化層結構表現出較高的氧訊號,而氧的存在可能降低銀表面能,導致銀或合金中銀成分在局部位置產生重組與團聚。此外,銀合金薄膜的初始粗糙度偏高,也會進一步促使局部結構晶粒成長。儘管如此,其團聚程度明顯低於純銀結構,整體仍維持良好之接合完整性,進一步驗證其具潛力的接合強度與應用價值。
經過驗證,本研究系統性展示搭配金屬鈍化層的鈷對鈷低溫接合結構,在不需高溫的情況下即可實現優異的機械與電性整合,並成功應用於晶圓與晶片層級,為未來高密度先進封裝與三維積體電路應用中,提供一項具備技術潛力與實務可行性的金屬接合解決方案。
This thesis proposes cobalt (Co) as a potential alternative to copper for low-temperature bonding applications. Cobalt offers several advantages, including superior electromigration resistance, shorter electron mean free path, and better performance in narrow linewidth interconnects. However, Co bonding faces similar challenges as Cu, such as surface oxidation and limited diffusion ability, especially at low temperatures. This work introduces metal passivation layers of silver (Ag) and Ag alloy (Ag-Pd-Cu, APC) to overcome these barriers to enhance the Co-Co bonding process under reduced thermal budgets.
This study first investigated the low-temperature Co-Co bonding behavior using a 10 nm Ag passivation layer. The bonding quality and electrical performance were evaluated and compared with non-passivated structures. The results showed that the Ag passivation layer effectively reduced Co surface roughness and improved bonding quality, enabling successful bonding at 150 °C with mechanical strength exceeding 5 MPa. At 200 °C, the structure achieved a specific contact resistance on the order of 10⁻⁷ Ω·cm², indicating excellent electrical conductivity and stable interface quality.
Two optimization strategies were explored to further enhance the bonding structure: using an Ag alloy (APC) and thinning the Ag layer to 3 nm. The APC passivation layer exhibited superior bonding strength compared to pure Ag structures, maintained conduction even at 150 °C, and showed stable electrical behavior under low-temperature conditions. On the other hand, reducing the Ag thickness to 3 nm also enabled bonding at 150 °C, with contact resistance remaining at the 10⁻⁷ Ω·cm² level, exhibiting comparable conductivity to the APC structure.
Further analyses using X-ray photoelectron spectroscopy (XPS) and transmission electron microscopy (TEM) were conducted to investigate the diffusion behavior and interfacial characteristics after bonding. XPS depth profiling revealed that both Ag and APC effectively suppressed oxidation and promoted Co atom diffusion, with the 3 nm Ag structure showing the most significant diffusion extent. TEM images confirmed that the APC-passivated interface was more stable and continuous, with less agglomeration, thereby enhancing mechanical and electrical properties. However, partial agglomeration was still observed in the APC structure. XPS results indicated a relatively high oxygen signal in the APC layer. The presence of oxygen likely reduced the surface energy, promoting silver redistribution and localized agglomeration. In addition, the higher initial surface roughness of the APC film may have contributed to localized grain growth. Nonetheless, the degree of agglomeration was lower than that of the pure Ag structure, and overall bonding integrity remained high, validating the potential bonding strength and practical value of the APC approach.
This work systematically demonstrates a Co-Co low-temperature bonding structure enhanced by metal passivation layers. Excellent mechanical and electrical integration was achieved at both wafer and chip levels without requiring high temperatures. These results provide a technically feasible and industrially promising bonding solution for future high-density 3D integrated circuits and advanced packaging applications.
This study first investigated the low-temperature Co-Co bonding behavior using a 10 nm Ag passivation layer. The bonding quality and electrical performance were evaluated and compared with non-passivated structures. The results showed that the Ag passivation layer effectively reduced Co surface roughness and improved bonding quality, enabling successful bonding at 150 °C with mechanical strength exceeding 5 MPa. At 200 °C, the structure achieved a specific contact resistance on the order of 10⁻⁷ Ω·cm², indicating excellent electrical conductivity and stable interface quality.
Two optimization strategies were explored to further enhance the bonding structure: using an Ag alloy (APC) and thinning the Ag layer to 3 nm. The APC passivation layer exhibited superior bonding strength compared to pure Ag structures, maintained conduction even at 150 °C, and showed stable electrical behavior under low-temperature conditions. On the other hand, reducing the Ag thickness to 3 nm also enabled bonding at 150 °C, with contact resistance remaining at the 10⁻⁷ Ω·cm² level, exhibiting comparable conductivity to the APC structure.
Further analyses using X-ray photoelectron spectroscopy (XPS) and transmission electron microscopy (TEM) were conducted to investigate the diffusion behavior and interfacial characteristics after bonding. XPS depth profiling revealed that both Ag and APC effectively suppressed oxidation and promoted Co atom diffusion, with the 3 nm Ag structure showing the most significant diffusion extent. TEM images confirmed that the APC-passivated interface was more stable and continuous, with less agglomeration, thereby enhancing mechanical and electrical properties. However, partial agglomeration was still observed in the APC structure. XPS results indicated a relatively high oxygen signal in the APC layer. The presence of oxygen likely reduced the surface energy, promoting silver redistribution and localized agglomeration. In addition, the higher initial surface roughness of the APC film may have contributed to localized grain growth. Nonetheless, the degree of agglomeration was lower than that of the pure Ag structure, and overall bonding integrity remained high, validating the potential bonding strength and practical value of the APC approach.
This work systematically demonstrates a Co-Co low-temperature bonding structure enhanced by metal passivation layers. Excellent mechanical and electrical integration was achieved at both wafer and chip levels without requiring high temperatures. These results provide a technically feasible and industrially promising bonding solution for future high-density 3D integrated circuits and advanced packaging applications.
所屬典藏
電子物理學系引用此條目
Cheng, L.-H. (2025). Investigation of Low-temperature Co-Co Bonding with Metal Passivation for Advanced Packaging and Ultra-Fine Pitch Applications. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/86359
引用文字依 APA 第 7 版格式自動產生,使用前請再核對。