銅晶粒尺寸與表面取向對低溫銅-銅接合之影響

Impact of Cu Grain Size and Surface Orientation on the Low Temperature Cu-Cu Bonding

檔案

日期

2025

類型

語言

中文

摘要

本研究系統性探討銅晶粒尺寸與取向對低溫銅-銅直接接合之影響。首先,藉由調整電鍍添加劑濃度以控制銅薄膜表面 (111) 晶面比例,當添加劑濃度提升,非 (111) 晶面的成長受到有效抑制,並進一步促進 (111) 晶面的生成。結果顯示當 (111) 比例達 61.5% 時,可顯著提升接合介面品質與剪力強度,透過低表面(111)與高表面(111)比例進行低溫接合時,接合強度提升至原先的三倍,且破壞模式由介面破壞轉為矽基板破壞,顯示高 (111) 比例可促進晶粒成長與介面結構轉變,進而提升接合強度。其次,本研究成功製備晶粒尺寸低於 100 nm 的奈米晶銅,其展現出優異的熱穩定性與機械性能,剪力強度超過 30 MPa,破壞位置位於矽基板,證實其具備可靠的低溫接合能力。最後,藉由奈米級介面孔洞的定量分析,比較奈米晶銅與奈米雙晶銅的差異,結果顯示奈米晶銅接合介面孔洞比例僅 1.8%,不到奈米晶銅的一半,歸因於奈米晶銅較高的熱膨脹與潛變速率特性,能於接合過程中有效排除介面殘留氣體。然而,在 250 ℃下則觀察到孔洞粗化與總面積增加的現象,推測與空孔於晶界成核並析出有關。
綜合而言,本研究證明銅表面(111)比例與晶粒尺寸對低溫銅銅接合強度與介面完整性具有關鍵影響,高 (111) 比例與奈米晶銅均能顯著提升接合可靠度,其中奈米晶銅更展現抑制介面孔洞生成的優勢,對先進封裝發展具重要潛力。
This study systematically investigates the effects of Cu grain size and orientation on low-temperature Cu-Cu direct bonding. First, by adjusting the concentration of electroplating additives to control the surface (111) ratio of Cu films, it was found that increasing additive concentration effectively suppressed the growth of non-(111) planes while promoting the formation of (111) planes. The results showed that when the (111) ratio reached 61.5%, the interfacial quality and shear strength were significantly improved. When bonding Cu films with low and high surface (111) ratios, the bonding strength increased by a factor of three, and the fracture mode shifted from interfacial failure to Si substrate failure, indicating that a high (111) ratio facilitated grain growth and interfacial structural transformation, thereby enhancing bonding strength. Second, nanocrystalline Cu (NC-Cu) films with grain sizes below 100 nm were successfully fabricated, exhibiting excellent thermal stability and mechanical performance. Shear tests demonstrated bonding strengths exceeding 30 MPa with fracture occurring in the Si substrate, confirming their reliable low-temperature bonding capability. Finally, quantitative analysis of nanoscale interfacial voids was conducted to compare NC-Cu and nanotwinned Cu (NT-Cu). The results revealed that the void area ratio at the NC-Cu bonding interface was only 1.8%, less than half that of NT-Cu, which can be attributed to the higher thermal expansion and creep rate of NC-Cu that effectively expelled residual interfacial gases during bonding. However, at 250 °C, typical void coarsening and an increase in total void area were observed, which are likely related to void nucleation and precipitation along grain boundaries.
In summary, this study demonstrates that both the surface (111) ratio and grain size of Cu play critical roles in determining the bonding strength and interfacial integrity of low-temperature Cu–Cu joints. A high (111) ratio and NC-Cu were both shown to significantly improve bonding reliability, with NC-Cu further exhibiting superior suppression of interfacial void formation, highlighting its potential for advanced packaging applications.
顯示完整詮釋資料 統計資料

引用此條目

黃建元 (2025). 銅晶粒尺寸與表面取向對低溫銅-銅接合之影響. https://thesis.lib.nycu.edu.tw/handle/20.500.14371/87259

BibTeX RIS

引用文字依 APA 第 7 版格式自動產生,使用前請再核對。

分享

永久網址:https://thesis.lib.nycu.edu.tw/handle/20.500.14371/87259