利用暫態液相法接合鋁/鈦平板
Transient liquid phase bonding of aluminum / titanium plate
摘要
鈦具有優異的機械性能,使用於航太工業、生物醫學等方面已大有佳績,但是由於鈦本身昂貴不已、強度高且不容易加工成形,故可以結合鋁合金已利於達到成本降低、輕量化、易於加工之雙贏局面。然而,兩金屬之熱膨脹係數、熔點、導電性、導熱性等等各項物理性質差異甚大,故很難接合為一體。本研究利用雙電子槍蒸鍍鎳、銅、矽、鍺各300奈米為中間層以利於暫態液相接合法來接合兩金屬,並全程使用氬氣保護氣氛防止氧化,該方法取決於鋁金屬與中間蒸鍍層之間的共晶反應在接合界面處形成薄的連續液體來潤濕鋁金屬表面,即可在較低溫之情況使鋁與鈦接合並且形成Al3Ti中間反應相化合物,該反應還具有能夠除去表面氧化物的優點。
本研究利用使用X-射線繞射分析(XRD)來鑑定相、熱場發射掃描電子顯微鏡和能量散射光譜儀(FESEM / EDS),穿透式電子顯微鏡和能量散射光譜儀(TEM / EDS)觀察Al / Ti反應界面微觀組織,並且使用超音波掃描顯微鏡(SAT)來分析鈦/鋁接合界面之孔隙分布,也利用拉伸試驗來測試兩金屬之接合強度以及彎曲試驗來測量彎曲模數,結果為沉積鎳元素於鋁金屬表面的結果皆優於其餘三者,沉積鎳為共晶元素可使鋁與鈦在氬氣一大氣壓氣氛580°C下完成,且孔隙率低至1.56%、剪應力強度高至37 MPa、彎曲模數高至55 GPa。
本研究利用使用X-射線繞射分析(XRD)來鑑定相、熱場發射掃描電子顯微鏡和能量散射光譜儀(FESEM / EDS),穿透式電子顯微鏡和能量散射光譜儀(TEM / EDS)觀察Al / Ti反應界面微觀組織,並且使用超音波掃描顯微鏡(SAT)來分析鈦/鋁接合界面之孔隙分布,也利用拉伸試驗來測試兩金屬之接合強度以及彎曲試驗來測量彎曲模數,結果為沉積鎳元素於鋁金屬表面的結果皆優於其餘三者,沉積鎳為共晶元素可使鋁與鈦在氬氣一大氣壓氣氛580°C下完成,且孔隙率低至1.56%、剪應力強度高至37 MPa、彎曲模數高至55 GPa。
Titanium has excellent mechanical properties and has been used in aerospace, biomedical applications. However, titanium is expensive and difficult to be machined due to its high strength. Thus, it is possible to join the aluminum, which is low cost, light weight, and easy processing, to form a bilayer structure of metals. The physical properties of the aluminum and titanium, such as thermal expansion coefficient, melting point, electrical conductivity, thermal conductivity, etc., are great different, so it is difficult to bond together.
In this study, dual E-Gun evaporation system were used to evaporate nickel, copper, silicon and germanium each 300 nm as an intermediate layer to facilitate the transient liquid phase (TLP) bonding method to bond the aluminum and titanium. In order to prevent the oxidation after bonding, the samples will be annealed at the atmosphere of argon gas. The samples will be used X-ray diffraction analysis (XRD) to identify the reactional phases. The thermal field emission scanning electron microscopy and energy scatter spectrometer (FESEM / EDS) and transmission electron microscopy and energy scatter spectrometer (TEM / EDS) will be performed to observe the microstructure of the titanium/aluminum reaction and the scanning acoustic tomography (SAT) will be used to analyze the pore distribution of the titanium/aluminum joint. The shear and bending strength are used to evaluate the joint strength and bending modulus of the two metals. The results indicated the aluminum is bonded to the titanium at a lower temperature and formed an Al3Ti intermediate reaction phase compound. The deposition of nickel on the aluminum metal to join titanium possessed the best bonding properties than that of copper, silicon, and germanium. The void distribution, shear strength, and bending modulus of the aluminum/titanium plate with nickel film were measured as low as 1.56%, 37 MPa, and 55 GPa, respectively.
In this study, dual E-Gun evaporation system were used to evaporate nickel, copper, silicon and germanium each 300 nm as an intermediate layer to facilitate the transient liquid phase (TLP) bonding method to bond the aluminum and titanium. In order to prevent the oxidation after bonding, the samples will be annealed at the atmosphere of argon gas. The samples will be used X-ray diffraction analysis (XRD) to identify the reactional phases. The thermal field emission scanning electron microscopy and energy scatter spectrometer (FESEM / EDS) and transmission electron microscopy and energy scatter spectrometer (TEM / EDS) will be performed to observe the microstructure of the titanium/aluminum reaction and the scanning acoustic tomography (SAT) will be used to analyze the pore distribution of the titanium/aluminum joint. The shear and bending strength are used to evaluate the joint strength and bending modulus of the two metals. The results indicated the aluminum is bonded to the titanium at a lower temperature and formed an Al3Ti intermediate reaction phase compound. The deposition of nickel on the aluminum metal to join titanium possessed the best bonding properties than that of copper, silicon, and germanium. The void distribution, shear strength, and bending modulus of the aluminum/titanium plate with nickel film were measured as low as 1.56%, 37 MPa, and 55 GPa, respectively.