溫度變化對錫銀銲錫可靠度與微結構之影響
Effect of thermal treatment on the reliability and the microstructure of SnAg solder
摘要
In this study, the difference between tin-silver solder concentration in Cu/Sn-Ag pillar is discussed, the height of copper part is 70 um, and tin-silver part is 30um, we observethe multiple samples
(1wt%/2wt%/3wt% Sn-Ag) microstructure after various reliability test condition, include 1 to 3 times 260oC reflow, -65+1500oC thermal cycling, 1250oC and 1500oC high temperature storage test, -65+150oC and -55oC+125oC, and see if the 3 different concentration undergoes differnet intermetallic growing mechanism. The samples were then conducted shear test, observed the failure mode of rupture surface by cross-section and discuss the shear force effect.
After high temperature test, the IMCs (intermetallic compounds) become thicker over time. However the pin-holes, cracks, ruptures are'nt growing in intermetallic compound by SEM (scanning electronic microscope) cross-section observation.
The reliability test results also show the IMCs growing behaviour are similar in various concentration above, the interface between both side of IMCs after shear test are simlar either. The rupture mechanism of shear test is the extension of interior crack in Sn-Ag solder instead of abnormal brittle fracture mechanism. In the copper part, we analyze the plating copper shear test, besides the shear force is normal, all fracture part occured in the copper. Furthermore, we found the hardness obviously increase over reflow times when Ag concentration raise in hardness test. It suggest that Ag concentration is positive to the SA hardness.
(1wt%/2wt%/3wt% Sn-Ag) microstructure after various reliability test condition, include 1 to 3 times 260oC reflow, -65+1500oC thermal cycling, 1250oC and 1500oC high temperature storage test, -65+150oC and -55oC+125oC, and see if the 3 different concentration undergoes differnet intermetallic growing mechanism. The samples were then conducted shear test, observed the failure mode of rupture surface by cross-section and discuss the shear force effect.
After high temperature test, the IMCs (intermetallic compounds) become thicker over time. However the pin-holes, cracks, ruptures are'nt growing in intermetallic compound by SEM (scanning electronic microscope) cross-section observation.
The reliability test results also show the IMCs growing behaviour are similar in various concentration above, the interface between both side of IMCs after shear test are simlar either. The rupture mechanism of shear test is the extension of interior crack in Sn-Ag solder instead of abnormal brittle fracture mechanism. In the copper part, we analyze the plating copper shear test, besides the shear force is normal, all fracture part occured in the copper. Furthermore, we found the hardness obviously increase over reflow times when Ag concentration raise in hardness test. It suggest that Ag concentration is positive to the SA hardness.
在本實驗,探討銅柱(Cu/SnAg)中不同錫銀焊錫濃度主要銅高度70um錫銀銲料30um,濃度1wt%/2wt&/3wt%-SnAg使用260C 1-3次迴焊、-65+1500C溫度循環、1250C 及1500C高溫儲存及溫度循環(-65C+150C/-55C+125C)等可靠度測試後,觀察不同銀濃度金屬化合物之微結構變化,經由三種不同錫銀銲錫濃度的介金屬成長機制,並進行錫銀銅界面的推力測試,觀察剖面比較與推力及破裂失效面探討,並探討錫銀焊錫濃度對抗剪應力強度(Shear strength)之影響。
經由高溫測試,隨可靠度時間讀點增加,不同錫銀銲錫濃度的介金屬化合物厚度皆有增長。以SEM進行剖面觀察觀察微結構,金屬化合物介面間未觀察孔洞、裂縫、破裂,等增長。
不同的錫銀焊錫濃度試片,經可靠度的實驗後,雖然錫銀銲錫濃度不同,但IMC成長行為趨勢相近,推力測試的介金屬化合物界面結果,趨勢也是相近的,之後採用光學顯微鏡觀察錫銀焊錫剪應力測試破裂面觀察,觀察出所有的破裂機制發生在錫銀銲錫內部破裂併延伸,並無分析到異常的脆性破裂機制。並測試分析其電鍍銅剪應力強度,銅的推力測試結果為正常,光學顯微鏡觀察銅剪力測試破裂面,可發現所有的破裂機構全發生在銅破裂。
硬度測試中,試驗結果顯示Ag濃度越高,硬度隨迴銲次數加就越明顯,表示銀濃度對SA硬度變化有影響。
經由高溫測試,隨可靠度時間讀點增加,不同錫銀銲錫濃度的介金屬化合物厚度皆有增長。以SEM進行剖面觀察觀察微結構,金屬化合物介面間未觀察孔洞、裂縫、破裂,等增長。
不同的錫銀焊錫濃度試片,經可靠度的實驗後,雖然錫銀銲錫濃度不同,但IMC成長行為趨勢相近,推力測試的介金屬化合物界面結果,趨勢也是相近的,之後採用光學顯微鏡觀察錫銀焊錫剪應力測試破裂面觀察,觀察出所有的破裂機制發生在錫銀銲錫內部破裂併延伸,並無分析到異常的脆性破裂機制。並測試分析其電鍍銅剪應力強度,銅的推力測試結果為正常,光學顯微鏡觀察銅剪力測試破裂面,可發現所有的破裂機構全發生在銅破裂。
硬度測試中,試驗結果顯示Ag濃度越高,硬度隨迴銲次數加就越明顯,表示銀濃度對SA硬度變化有影響。